Чат с нами, при поддержке LiveChat

Buna-N 70 против 90 по Шору: всегда ли твёрже значит лучше?

Кольцо 90 Shore A — это не кольцо 70 Shore A с большим запасом. Что даёт дополнительный технический углерод в стойкости к выдавливанию, чем он обходится в остаточной деформации сжатия и морозостойкости, и почему шкала A заканчивается на 90.

Поделиться этой публикацией

Every seal catalogue lists NBR in two grades: 70 Shore A and 90 Shore A. The 90 costs more, appears in the “high pressure” section, and gets specified whenever an engineer wants a margin. That habit produces failures that look like material problems and are actually selection problems — a 90 Shore A ring that will not seal at 3 bar on a machined cover, or a 70 Shore A ring that nibbles into the gap at 250 bar. This article separates the two grades by what the number changes inside the compound, then sets out where each one earns its place.

Seal quality control bench with durometer, caliper and nitrile O-ring samples

What the number measures, and what it does not

Shore A hardness is indentation resistance, measured with a spring-loaded conical indentor under ASTM D2240 or ISO 48-4. It is not modulus, not stiffness of the assembled joint, and not a strength rating. Two compounds at the same 70 Shore A can differ by 20 to 30 percent in elastic modulus depending on polymer and filler system.

In an NBR compound, hardness is raised mainly by carbon black. A 70 Shore A general-purpose nitrile might carry 40 to 50 phr of carbon black; a 90 Shore A grade carries roughly 70 to 90 phr, sometimes with a harder reinforcing grade and less plasticizer. That change in filler loading is what alters every other property in the table below — not the hardness number itself.

The trade you are making

СвойствоNBR 70 Shore ANBR 90 Shore AWhy the change happens
Extrusion resistance in a wide gapModerate; needs a backup ring above roughly 100–150 barHigh; tolerates larger gaps at the same pressureHigher modulus resists being pushed into the clearance
Compression set, 22 h at 100 °C (ASTM D395 B)Typically 15–30%Typically higher, often 25–40% for the same cureFiller loading restricts elastic recovery; less rubber phase to store strain energy
Относительное удлинение при разрыве250–400%Often 150–200%, and 150% is a common minimum in supplier dataSame filler effect; the compound has less stretch before rupture
Низкотемпературная гибкостьService to about −40 °C for a good low-temperature gradeUsually 5–10 °C worse for the same base polymerFiller and lower plasticizer content raise the glass transition region
Conformability to a rough or slightly uneven surfaceGood; seals at lower compressionPoor; needs a smoother face and more squeezeLess flow into surface valleys at the same seating force
Sealing force on the hardwareLower; kinder to plastic covers and thin flangesHigher; can bow a stamped cover or creep a plastic housingHigher modulus at the same compression ratio
Tear and abrasion resistanceAdequateBetter in clean abrasive duty, worse once a nick startsHigher stiffness resists wear; lower elongation concentrating stress at a defect

Two rows deserve emphasis because they run against the usual “harder is stronger” instinct. Compression set and conformability both get worse at 90 Shore A, and both are what a static seal actually depends on. A seal does not hold pressure by being hard; it holds pressure by staying deformed against the surface for years.

Aged nitrile O-ring with cracks next to a new O-ring of the same size

Where 90 Shore A earns its price

Four situations justify the harder grade, and in each the mechanism is the same: the seal has to resist a force that would deform a softer compound.

Static high pressure with a real gap. Above roughly 150–200 bar, a 70 Shore A O-ring starts to extrude into the clearance between gland and bore. A 90 Shore A ring pushes that threshold up, but it does not remove it. Above 300 bar, the answer is a backup ring or a changed groove, not a harder compound — the сравнение материалов опорных колец covers which polymer to put behind the seal.

Rotary and oscillating duty with abrasive contamination. Higher hardness reduces wear rate where grit is present and the seal cannot be protected. This is the reason 90 Shore A NBR appears in some oil seal and wiper specifications for construction equipment.

Large cross-sections under high squeeze. A 6.99 mm cross-section ring in a 25% compression groove carries a large volume of rubber. The softer grade can shear internally at the groove corners during assembly; the harder grade resists that.

Metric and inch hardware with generous tolerances. Where the groove depth varies by ±0.05 mm across a production run, a harder ring varies less in sealing force — which helps consistency, at the cost of the conformability described earlier.

Where 70 Shore A wins, and why engineers forget it

The default grade is the default for a reason. It conforms to a surface that is not perfect, it seals at lower compression, it recovers better after long compression, and it keeps working at low temperature. Those four properties decide most static sealing jobs in pumps, gearboxes, valve covers, filter housings and pneumatic equipment.

Three specific cases where 90 Shore A is the wrong call:

Thin or plastic hardware. A stamped steel cover or a moulded PA66 housing deflects under the seating force of a 90 Shore A ring. The joint opens at one side, the seal follows the gap, and the leak appears at the bolt furthest from the first one tightened.

Cold start conditions. A 90 Shore A NBR at −25 °C behaves closer to a rigid gasket than an elastomer. Equipment that starts cold and pressurises before warm-up will leak until the housing reaches operating temperature.

Rough or as-machined surfaces. A turned cover with Ra 3.2 µm and visible tool marks needs the softer compound to flow into the profile. Harder rubber bridges the peaks and leaves a leak path in the valleys, and the groove surface finish requirements explain what the mating face should measure before hardness is used to compensate for it.

The measurement trap at the top of the scale

Hardness testing is the cheapest incoming inspection a seal buyer can run, and the least reliable if done carelessly. Four rules matter at 90 Shore A:

The scale runs out. ASTM D2240 recommends switching to Shore D when Shore A reads above 90, and back to Shore A when Shore D reads below 20. A “90 Shore A” compound is therefore measured at the top edge of the scale, where the spring force is high and the reading compresses. Nominal 90 with a ±5 tolerance spans 85 to 95, and readings above 90 on the A scale carry more uncertainty than readings at 70.

IRHD and Shore A diverge up here. In the 30–80 range the two scales agree within about ±2 points. Above 90 Shore A, IRHD typically reads 2–5 points higher than Shore A for the same sample. A supplier quoting IRHD 93 and a buyer measuring Shore A 88 are describing the same part.

Specimen thickness. The test needs at least 6 mm of rubber under the indentor, or the anvil underneath adds stiffness and inflates the reading. An O-ring of 3.53 mm cross-section measured on a bench top is not a valid test; stack it, or use a micro IRHD instrument designed for thin sections.

Instantaneous versus delayed reading. Values taken at 1 second and at 15 seconds differ by several points on viscoelastic rubber. State the delay in the specification, or two labs will disagree about a conforming batch. The ASTM D2240 standard sets out the timing, and the Apple Rubber technical library has a practical comparison of durometer and IRHD readings for common seal compounds.

What actually changes when you jump 20 points

Specification fieldEffect of moving from 70 to 90 Shore AWhat to re-check
Compression ratioSame ratio, higher force; recovery slowerGroove depth and hardware stiffness; consider dropping from 25% to 20% squeeze
Surface finishLess tolerance of roughnessMating face to Ra 1.6 µm or better for dynamic duty
УстановкаHarder to stretch over a piston without scoringAssembly lubricant, tapered lead-in, and whether the ring can be heated
Low-temperature ratingStart temperature shifts up 5–10 °CCold start procedure, and whether a low-temperature plasticizer grade is available
Compression set limitWorse by roughly 5–10 percentage pointsWhether the joint is opened for service; if yes, keep 70 or change polymer
CostSlightly higher compound cost, same toolingNothing — this is the smallest factor in the decision

There is a third option that engineers underuse: stay at 70 Shore A and change the geometry instead. A PTFE or PEEK backup ring on the low-pressure side, a smaller extrusion gap by tightening the bore tolerance, or a change from O-ring to a profile seal with an anti-extrusion shoulder all solve the same problem without paying the compression set penalty. The compression set mechanism is worth reading before any hardness increase is signed off, because set is what turns a seal into a leak two years later. Where pressure runs past 400 bar, no elastomer hardness answers it; the seal architecture changes, and spring-energized designs from specialists such as Bal Seal Engineering are designed for that range.

Nitrile and EPDM O-rings with oil and water samples for compatibility testing

Material choice often matters more than the number

If the application is hot oil at 120 °C with a 250 bar pressure spike, a 90 Shore A NBR may still be the wrong answer, because the polymer is at its temperature limit and compression set will dominate. An 80 Shore A HNBR at the same geometry usually outlasts it. Distributor datasheets from houses such as ERIKS print Shore A and IRHD side by side for the same compound, which is a quick way to see how much of a hardness argument is a units argument. Our note on NBR versus HNBR sets out where the hydrogenated polymer earns its premium, and the comparison of NBR against EPDM covers the fluid side of the same decision.

Frequently asked questions

Is 90 Shore A always better for high pressure?

No. It raises the extrusion threshold but worsens compression set and conformability. Above roughly 300 bar, a backup ring or a profile seal does more than 20 points of hardness. Hardness is a supplement to anti-extrusion design, not a replacement for it.

Can I use 90 Shore A in a standard AS568 groove?

The groove dimensions are the same; the force is not. Check the hardware stiffness and the surface finish first. If the cover is thin, the groove is in plastic, or the surface is as-machined, keep 70 Shore A or reduce groove depth to lower the seating force.

Why does my supplier’s 90 Shore A measure 85 on my durometer?

Both may be correct. Readings above 90 on the A scale are less reliable, IRHD reads higher than Shore A in that range, and a 3.53 mm cross-section measured on a bench top gives an inflated value. Stack the rings to 6 mm and specify the reading delay before rejecting a batch.

Does harder rubber last longer?

In abrasive dynamic duty, often yes. In static sealing, usually no — compression set and conformability decide life, and both degrade as hardness rises. Match the grade to the failure mode you actually see, not to the one that sounds worse.

What about 80 Shore A?

It is a legitimate middle grade and often the correct answer for high-pressure static joints with good surface finish. It is less commonly stocked, so confirm availability before writing it into a drawing that a distributor has to fill for the next five years.

Наши nitrile and fluorocarbon O-ring range is molded in 70, 80 and 90 Shore A as standard, and 90 Shore A rings are quoted against the same tooling as the 70 grade — the difference is compound, not mould.

Подробнее

Buna-N 70 против 90 по Шору: всегда ли твёрже значит лучше?

Кольцо 90 Shore A — это не кольцо 70 Shore A с большим запасом. Что даёт дополнительный технический углерод в стойкости к выдавливанию, чем он обходится в остаточной деформации сжатия и морозостойкости, и почему шкала A заканчивается на 90.

Соответствие уплотнений требованиям REACH, RoHS и Prop 65: какие документы должны подготовить импортеры

Три режима регулирования — три разных юридических вопроса. Где на самом деле сосредоточен риск SVHC в резиновой смеси, как ограничения RoHS для однородных материалов распространяются на уплотнение, и десять документов, которые нужно запросить до отправки контейнера.