A drawing arrives from a European customer showing a 25.0 × 3.55 mm O-ring. The American plant has AS568 rings on the shelf. Someone asks whether a -214 is “close enough.” The answer is: the cross-sections differ by 0.02 mm and the gland decides — sometimes yes, sometimes no, and the difference is tolerances and squeeze, not arithmetic. Converting between AS568 and metric O-ring systems is straightforward once you know which system you are actually looking at, and error-prone when you do not.

Step One: Identify Which “Metric” You Are Holding
Three different things get called metric O-rings, and the cross-section is the fastest fingerprint:
- AS568 sizes written in millimeters. Cords of 1.78, 2.62, 3.53, 5.33 and 6.99 mm are inch-based AS568 sections (1/16, 3/32, 1/8, 3/16, 1/4 inch) expressed in metric units. The part is identical to the imperial ring, tolerances included.
- ISO 3601-1 metric sizes. Cords of 1.80, 2.65, 3.55, 5.30 and 7.00 mm form the international metric series. Each sits next to an AS568 cord but is not the same part.
- JIS B 2401 (Japanese) sizes. Cords of 1.9, 2.4, 3.5, 5.7 and 8.4 mm form a separate system with its own number catalog — the Japanese standard’s cross-sections mostly do not overlap AS568 cleanly except at 3.5 mm.
Read the cross-section on the drawing or the ring before anything else. A 3.53 mm cord means AS568; 3.55 mm means ISO 3601; 3.5 mm almost certainly means JIS. Confusing the three is the single most common conversion error we see in RFQs that arrive with mixed-unit drawings. If the incoming ring arrives unlabeled, the same cross-section and ID discipline applies as for any ring in our rubberen O-ring- en X-ring-rige.
| Standard | Standard cross sections (mm) | Size notation | Example |
|---|---|---|---|
| AS568 (SAE) | 1.78, 2.62, 3.53, 5.33, 6.99 (+ 900 boss series) | 3-digit dash number (catalog lookup) | -214 |
| ISO 3601-1 | 1.80, 2.65, 3.55, 5.30, 7.00 | Group letter + ID in tenths of mm | C0250 = 25.0 × 3.55 mm |
| JIS B 2401 | 1.9, 2.4, 3.5, 5.7, 8.4 | Catalog number, not a dimension | S25 (25 × 3.5) |
How AS568 Dash Numbers Encode Size
The dash number is a catalog lookup, not a formula. The first digit names the cross-section series — 0xx through 4xx — and the remaining digits index position within that series. Two rules worth memorizing:
- -001, -002 and -003 sit below the 1/16-inch series with cords of 0.040, 0.050 and 0.060 in (1.02, 1.27, 1.52 mm) and have no ISO 3601 counterpart at all.
- The -901 to -932 series is separate: 20 straight-thread tube-fitting boss gaskets that ISO 3601-1 does not carry. Metric fittings use ISO 6149 threads instead, so a “metric equivalent” of a boss gasket does not exist — the fitting standard changed, not just the ring.
A worked example: -214 reads as series 2 (3.53 mm cord), position 14, which is 24.99 mm ID × 3.53 mm CS. A European drawing calling out 25.0 × 3.55 mm (ISO C0250) is nearly the same ring — ID within a hundredth of a millimeter, cord 0.02 mm fatter. Whether the ISO ring can stand in for the AS568 ring depends on the gland, which we address below.
For the complete dash-number table with tolerances, see our AS568 O-ring sizes reference, and for the international system in depth, the ISO 3601 standard explainer.
How ISO 3601-1 Codes Are Written
ISO 3601-1 writes each size as a group letter followed by the inside diameter in tenths of a millimeter. Group letters map to cross-sections: A = 1.80, B = 2.65, C = 3.55, D = 5.30, E = 7.00 mm. So C0250 parses as group C (3.55 mm cord) + ID 25.0 mm. The code is self-describing, unlike the AS568 dash number, which requires the catalog.
JIS B 2401 goes the other way: its numbers are catalog indexes with no dimensional logic (P, G, S and V series for different duty classes), so a JIS number can only be converted with the size table. When a drawing carries a JIS number, our JIS B 2401 size guide lists the full mapping.
Tolerances: Why “Same Size” Is Not Always Interchangeable
Cross-section tolerances are similar between systems, but inside-diameter tolerances grow with size, and the two standards do not always put their tolerance bands in the same place. The ISO 3601-1 ID tolerance follows an approximate formula:
Δd₁ = ±((d₁0.95 × 0.009) + 0.11) mm
That is a dimension-model formula — tolerance grows with size in a smooth curve rather than in discrete jumps. Practical ranges from the same model:
| Inside diameter d₁ | Typical ID tolerance | AS568 cross-section series in that range |
|---|---|---|
| ≤ 15 mm | ±0.15 to ±0.20 mm | 0xx (1.78), 1xx (2.62) |
| 15–40 mm | ±0.20 to ±0.35 mm | 2xx (3.53), lower 3xx (5.33) |
| 40–100 mm | ±0.35 to ±0.60 mm | upper 3xx, lower 4xx (6.99) |
| 100–250 mm | ±0.60 to ±1.30 mm | upper 4xx |
AS568 tolerances are specified in inches per series and widen with size as well — roughly ±0.004 in on ID at the small end versus ±0.033 in in the 4xx series. The bands overlap the ISO ranges but do not coincide, which is why a substitution check must compare worst-case squeeze, not nominal sizes.
Can an ISO Ring Replace an AS568 Ring? The Gland Decides
Substitution is a squeeze-and-fill question, not a units question. Run both candidate rings through the gland arithmetic:
- Knip. Calculate the cross-section squeeze percentage the gland produces for each cord (3.53 vs 3.55 mm is a 0.6% difference in cord, which shifts squeeze by roughly a percentage point of squeeze depending on gland depth). Most static designs target squeeze that tolerates this; aggressive or marginal designs do not.
- Gland-folling. The fatter ISO cord fills more of the groove. If the AS568 design sits near the fill ceiling (keeping clearance for thermal expansion), the ISO ring can push it over.
- Stretch and ID fit. Compare worst-case IDs: ring stretched over a piston or compressed on a rod changes effective cross-section. The ID tolerance bands overlap but differ, so worst cases can differ even when nominal IDs match.
- Compound and hardness match. A conversion across standards usually crosses suppliers too. Hardness, compound and batch discipline should follow the same checks as any substitution — measure the incoming ring, do not trust the print, using the same technique as for any O-ring dimensional check.
If all four check out, the substitution is sound for static service. For dynamic service we recommend staying on the standard the gland was designed around; seal suppliers design lip interference and squeeze bands around a specific cord, and “nearly the same” is a smaller margin than a dynamic seal wants.

A Conversion Workflow for Mixed-Unit Drawings
When drawings, stock and suppliers disagree on units, this workflow keeps the process honest:
- Fingerprint the cross-section (1.78 vs 1.80 vs 1.9 mm class) to identify the system the designer intended.
- Convert notation properly: dash numbers via the catalog table; ISO codes by group letter + tenths; JIS numbers via size table only.
- Search your own shelf in the original system first. A 25 × 3.55 mm callout has no exact AS568 twin; the nearest dash is -214 (24.99 × 3.53), and whether that is acceptable is a gland calculation, not a lookup.
- Verify worst-case squeeze and fill with both rings’ full tolerance bands before approving a substitution.
- Document the decision. Note on the drawing or BOM which part number supersedes which, so the next buyer does not repeat the analysis or, worse, reverse it.
Suppliers maintain reference tables that pair each ISO 3601 metric size with its nearest AS568 dash number — Precision Polymer Engineering’s published ISO 3601 size table is a good example — but note that responsible suppliers label these “nearest,” not “equivalent.” The print governs; the gland decides.
Two Traps Worth Naming
The 1.78 vs 1.80 trap. Calipers cannot reliably distinguish 1.78 from 1.80 mm cord, and neither can most incoming inspectors — which is fine, because a 0.02 mm difference matters at the gland, not the dock. What matters at the dock is that the documented system matches the gland design. If your receiving inspection measures 1.79 mm on a ring labeled 1.78, that is within tolerance for both systems; do not reject on it.
The round-number trap. A buyer asked for “25 by 3.5 mm” rings and received JIS-pattern 3.5 mm cord in an ISO-3601-designed gland — 0.05 mm of missing cord, a small squeeze shortfall, a slow weep that took weeks to trace. When converting, carry both decimal places to the end of the analysis. Rounding happens at the purchase order, never at the gland.

Wichtichste punten
- Cross-section is the fingerprint: 1.78/2.62/3.53/5.33/6.99 mm = AS568 in metric units; 1.80/2.65/3.55/5.30/7.00 mm = ISO 3601-1; 1.9/2.4/3.5/5.7/8.4 mm = JIS B 2401.
- AS568 dash numbers are catalog lookups, not formulas; ISO 3601-1 codes (letter + ID in tenths, e.g. C0250) are self-describing; JIS numbers require a size table.
- -001 to -003 and the -901 to -932 boss series have no metric counterparts — the substitution conversation ends before it starts.
- Tolerance bands differ between standards even when nominal sizes nearly match; approve substitution with worst-case squeeze and gland-fill calculations, not nominal dimensions.
- Nearest-size tables pair ISO sizes with AS568 dash numbers as a starting point — the gland decides, the print governs, and rounding belongs on the purchase order, not in the groove.