{"id":1697,"date":"2026-11-13T15:53:00","date_gmt":"2026-11-13T07:53:00","guid":{"rendered":"https:\/\/www.bosssealing.com\/?p=1697"},"modified":"2026-11-10T12:00:31","modified_gmt":"2026-11-10T04:00:31","slug":"200c-%e4%bb%a5%e4%b8%8a%e7%9a%84%e5%af%86%e5%b0%81%e4%bb%b6","status":"publish","type":"post","link":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/","title":{"rendered":"200 \u00b0C \u4ee5\u4e0a\u7684\u5bc6\u5c01\u4ef6\uff1aFKM\u3001FFKM\u3001PEEK \u8207\u77f3\u58a8\u9078\u9805\u6bd4\u8f03"},"content":{"rendered":"<p>\u4e00\u500b\u984d\u5b9a\u8010\u6eab 230 \u00b0C \u7684 O \u578b\u74b0\uff0c\u50f9\u9322\u5927\u7d04\u7b49\u65bc\u4e00\u676f\u5496\u5561\u3002\u5b83\u53ef\u4ee5\u627f\u53d7\u4e00\u500b\u73ed\u6b21\u7684\u58d3\u529b\uff0c\u6709\u6642\u751a\u81f3\u80fd\u6490\u4e00\u500b\u6708\u3002\u7136\u5f8c\u5b83\u5f9e\u6e9d\u69fd\u88e1\u53d6\u51fa\u4f86\u6642\u5df2\u7d93\u6241\u5e73\u3001\u786c\u5316\u3001\u908a\u7de3\u8b8a\u65b9\uff0c\u6cd5\u862d\u4e5f\u958b\u59cb\u5728\u87ba\u6813\u8655\u6ef2\u6f0f\u3002\u9298\u724c\u4e0a\u7684\u6eab\u5ea6\u5b8c\u5168\u6c92\u932f\u3002\u5931\u6548\u7684\u539f\u56e0\u662f\u505c\u7559\u5728\u8a72\u6eab\u5ea6\u7684\u6642\u6578\u3001\u7576\u6642\u5b58\u5728\u7684\u6d41\u9ad4\uff0c\u4ee5\u53ca\u6c92\u6709\u4eba\u554f\u904e\u9019\u7a2e\u5f48\u6027\u9ad4\u5728\u7d93\u6b77 4,000 \u500b\u9019\u6a23\u7684\u6642\u6578\u4e4b\u5f8c\u6703\u8b8a\u6210\u4ec0\u9ebc\u6a23\u5b50\u3002<\/p>\n<p>\u5728 200 \u00b0C \u4ee5\u4e0a\u5bc6\u5c01\uff0c\u4e0d\u662f\u4e00\u5834\u8cb7\u6750\u6599\u7684\u63a1\u8cfc\u7df4\u7fd2\u3002\u9019\u662f\u4e00\u5834\u71b1\u9810\u7b97\u7684\u6f14\u7b97\uff0c\u6d89\u53ca\u4e09\u500b\u8b8a\u6578\uff1a\u5bc6\u5c01\u4ecb\u9762\u7684\u9023\u7e8c\u6eab\u5ea6\u3001\u5728\u8a72\u6eab\u5ea6\u4e0b\u7684\u505c\u7559\u6642\u9593\uff0c\u4ee5\u53ca\u52a0\u901f\u6216\u963b\u6b62\u6c27\u5316\u7684\u5316\u5b78\u74b0\u5883\u3002\u9019\u4e09\u9805\u6293\u5c0d\u4e86\uff0c\u6750\u6599\u5019\u9078\u6e05\u55ae\u81ea\u7136\u5c31\u5beb\u5f97\u51fa\u4f86\u3002\u6293\u932f\u4e86\uff0cFFKM \u4e5f\u6703\u50cf\u4e00\u500b 0.30 \u7f8e\u5143\u7684 FKM \u74b0\u4e00\u6a23\uff0c\u5728\u540c\u6a23\u7684\u516d\u9031\u5167\u5931\u6548\u3002<\/p>\n<p>\u672c\u6307\u5357\u6bd4\u8f03\u56db\u7a2e\u771f\u6b63\u7528\u65bc 200 \u00b0C \u4ee5\u4e0a\u7684\u6750\u6599\u7cfb\u5217\u2014\u2014FKM\u3001FFKM\u3001PTFE\/PEEK \u4ee5\u53ca\u77f3\u58a8\u6216\u91d1\u5c6c\u2014\u2014\u5217\u51fa\u5340\u5206\u5b83\u5011\u7684\u6578\u64da\u3001\u6bcf\u4e00\u7a2e\u6240\u9700\u7684\u786c\u4ef6\u6539\u52d5\uff0c\u4ee5\u53ca\u7576\u5ba2\u6236\u628a\u9ad8\u6eab\u61c9\u7528 RFQ \u9001\u5230\u6211\u5011\u4f5b\u5c71\u5de5\u5ee0\u6642\uff0c\u6211\u5011\u6240\u63a1\u7528\u7684\u5de5\u4f5c\u6d41\u7a0b\u3002<\/p>\n<figure><img fetchpriority=\"high\" decoding=\"async\" src=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2026\/11\/a1_hero-2.jpg\" alt=\"\u9ad8\u6eab\u5bc6\u5c01\u5957\u4ef6\uff1a\u92fc\u677f\u4e0a\u7684\u68d5\u8272 FKM O \u578b\u74b0\u3001\u767d\u8272 PTFE \u74b0\u53ca PEEK \u64cb\u5708\" width=\"1536\" height=\"1024\" loading=\"eager\" \/><figcaption>\u56db\u500b\u7cfb\u5217\uff0c\u540c\u4e00\u689d\u6e9d\u69fd\uff1aFKM\u3001\u586b\u5145 PTFE\u3001PEEK \u548c\u5f48\u7c27\u84c4\u80fd\u74b0\u3002\u6bcf\u4e00\u7a2e\u5728 200 \u00b0C \u4ee5\u4e0a\u90fd\u6709\u4e0d\u540c\u7684\u5931\u6548\u65b9\u5f0f\u3002<\/figcaption><\/figure>\n<h2>200 \u00b0C \u5c0d\u5bc6\u5c01\u4ef6\u7a76\u7adf\u505a\u4e86\u4ec0\u9ebc<\/h2>\n<p>\u805a\u5408\u7269\u4e0d\u6703\u5728 200 \u00b0C \u7194\u5316\u3002\u5be6\u969b\u767c\u751f\u7684\u904e\u7a0b\u66f4\u6162\uff0c\u4e5f\u66f4\u6602\u8cb4\u3002\u56db\u7a2e\u6a5f\u5236\u540c\u6642\u9032\u884c\uff0c\u6700\u5148\u5b8c\u6210\u7684\u90a3\u4e00\u7a2e\u5c31\u6c7a\u5b9a\u4e86\u4f60\u7684\u4fdd\u990a\u9031\u671f\u3002<\/p>\n<p><strong>\u6c27\u5316\u8207\u4ea4\u806f\u786c\u5316\u3002<\/strong> \u6c27\u6c23\u653b\u64ca\u805a\u5408\u7269\u4e3b\u93c8\u4e26\u589e\u52a0\u4ea4\u806f\u3002\u6a61\u81a0\u6703\u8b8a\u786c\u3001\u5931\u53bb\u65b7\u88c2\u4f38\u9577\u7387\uff0c\u4e26\u5728\u58d3\u529b\u5faa\u74b0\u4e0b\u4e0d\u518d\u8cbc\u5408\u6e9d\u69fd\u3002\u4e00\u500b 70 Shore A \u7684\u81a0\u6599\u8001\u5316\u5f8c\u6e2c\u5f97 85 Shore A\uff0c\u770b\u8d77\u4f86\u4ecd\u7136\u50cf\u500b\u5bc6\u5c01\u4ef6\uff0c\u4f46\u884c\u70ba\u5df2\u7d93\u4e0d\u518d\u50cf\u4e86\u3002<\/p>\n<p><strong>\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u3002<\/strong> \u5bc6\u5c01\u4ef6\u5728\u8a2d\u8a08\u4e0a\u5c31\u6703\u88ab\u8b8a\u5f62\u2014\u2014\u901a\u5e38\u662f\u5176\u622a\u9762\u7a4d\u7684 15% \u5230 25%\u3002\u71b1\u6703\u8b93\u805a\u5408\u7269\u93c8\u6c38\u4e45\u5730\u5f9e\u9019\u7a2e\u8b8a\u5f62\u4e2d\u9b06\u5f1b\u51fa\u4f86\u3002\u4e00\u65e6\u6c38\u4e45\u8b8a\u5f62\u8d85\u904e\u7d04 40%\uff0c\u5bc6\u5c01\u7dda\u4e0a\u7684\u63a5\u89f8\u58d3\u529b\u5c31\u6703\u964d\u5230\u4f4e\u65bc\u5b83\u672c\u61c9\u963b\u64cb\u7684\u6d41\u9ad4\u58d3\u529b\uff0c\u65bc\u662f\u6ef2\u6f0f\u958b\u59cb\uff0c\u537b\u6c92\u6709\u4efb\u4f55\u53ef\u898b\u7684\u640d\u50b7\u3002<\/p>\n<p><strong>\u812b\u6c1f\u5316\u6c2b\u53cd\u61c9\u3002<\/strong> \u9019\u662f\u6c1f\u78b3\u6a61\u81a0\u7279\u6709\u7684\u73fe\u8c61\u3002\u5728\u84b8\u6c7d\u3001\u71b1\u6c34\u6216\u5f37\u9e7c\u4e2d\uff0c\u6eab\u5ea6\u9ad8\u65bc\u7d04 150 \u00b0C \u6642\uff0cFKM \u6703\u5f9e\u4e3b\u93c8\u4e0a\u5931\u53bb\u6c1f\u5316\u6c2b\u3002\u8868\u9762\u786c\u5316\u4e26\u8d77\u6ce1\uff0c\u4fb5\u8755\u5411\u5167\u63a8\u9032\u3002\u9019\u5c31\u662f\u70ba\u4ec0\u9ebc\u4e00\u500b\u5728\u4e7e\u6cb9\u4e2d 200 \u00b0C \u53ef\u7528\u7684\u5bc6\u5c01\u4ef6\uff0c\u5728\u98fd\u548c\u84b8\u6c7d\u4e2d 160 \u00b0C \u5c31\u6703\u5931\u6548\u3002<\/p>\n<p><strong>\u6a21\u91cf\u640d\u5931\u8207\u64e0\u51fa\u3002<\/strong> \u71b1\u6703\u8edf\u5316\u81a0\u6599\u3002\u5728 200 \u00b0C \u6642\uff0c\u4e00\u500b 75 Shore A \u7684 FKM \u74b0\u7684\u58d3\u7e2e\u6a21\u91cf\u5927\u6982\u53ea\u6709\u5b83\u5728 23 \u00b0C \u6642\u7684\u4e00\u534a\u3002\u540c\u6a23\u7684\u58d3\u529b\u548c\u540c\u6a23\u7684\u9593\u9699\uff0c\u5728\u51b7\u614b\u6642\u5b89\u5168\uff0c\u73fe\u5728\u537b\u6703\u628a\u6750\u6599\u64e0\u9032\u9593\u9699\u3002\u4e00\u65e6\u6709\u4e00\u5c0f\u584a\u6a61\u81a0\u88ab\u526a\u6389\uff0c\u9019\u500b\u5bc6\u5c01\u4ef6\u5c31\u5831\u5ee2\u4e86\u3002<\/p>\n<h2>\u56db\u7a2e\u771f\u6b63\u5728 200 \u00b0C \u904b\u884c\u7684\u7cfb\u7d71<\/h2>\n<p>\u5bc6\u5c01\u61c9\u7528\u4e2d\u7684\u71b1\u91cf\u4f86\u81ea\u56db\u7a2e\u4f86\u6e90\uff0c\u6bcf\u4e00\u7a2e\u90fd\u6709\u4e0d\u540c\u7684\u7279\u5fb5\u3002\u77e5\u9053\u81ea\u5df1\u9762\u5c0d\u7684\u662f\u54ea\u4e00\u7a2e\uff0c\u5c31\u80fd\u5728\u6253\u958b\u6578\u64da\u8868\u4e4b\u524d\u5148\u7e2e\u5c0f\u6750\u6599\u9078\u64c7\u7bc4\u570d\u3002<\/p>\n<p><strong>\u58d3\u7e2e\u8207\u6469\u64e6\u3002<\/strong> \u7a7a\u6c23\u58d3\u7e2e\u6a5f\u3001\u6db2\u58d3\u52d5\u529b\u55ae\u5143\u548c\u9f52\u8f2a\u7bb1\u6703\u52a0\u71b1\u6cb9\uff0c\u6cb9\u518d\u52a0\u71b1\u5bc6\u5c01\u4ef6\u3002\u5f80\u5fa9\u5f0f\u58d3\u7e2e\u6a5f\u6392\u6c23\u5074\u7684\u5bc6\u5c01\u4ef6\u5728\u6709\u6cb9\u7684\u60c5\u6cc1\u4e0b\uff0c\u7d93\u5e38\u627f\u53d7 180 \u5230 220 \u00b0C\u3002\u53ea\u8981\u6cb9\u662f\u7926\u7269\u6cb9\u6216 PAO \u57fa\uff0c\u4e14\u542b\u6c34\u91cf\u7dad\u6301\u5728\u4f4e\u6c34\u5e73\uff0cFKM \u5c31\u80fd\u5f88\u597d\u5730\u61c9\u4ed8\u3002<\/p>\n<p><strong>\u7d93\u7531\u91d1\u5c6c\u50b3\u5c0e\u7684\u88fd\u7a0b\u71b1\u3002<\/strong> 220 \u00b0C \u53cd\u61c9\u5668\u4e0a\u7684\u6cd5\u862d\u3001\u84b8\u6c7d\u96c6\u7ba1\u4e0a\u7684\u95a5\u84cb\u3001\u63db\u71b1\u5668\u7684\u901a\u9053\u84cb\u3002\u9019\u88e1\u5bc6\u5c01\u4ef6\u8655\u65bc\u91d1\u5c6c\u6eab\u5ea6\uff0c\u6d41\u9ad4\u53ef\u80fd\u5f88\u6eab\u548c\u2014\u2014\u98df\u54c1\u3001\u88fd\u85e5\u548c\u5316\u5de5\u64ac\u88dd\u8a2d\u5099\u4e2d\u5e38\u898b\u9019\u7a2e\u60c5\u6cc1\u3002\u50b3\u5c0e\u662f\u7a69\u5b9a\u4e14\u53ef\u9810\u6e2c\u7684\uff0c\u6240\u4ee5\u9023\u7e8c\u984d\u5b9a\u503c\u5c31\u662f\u6b63\u78ba\u7684\u8a2d\u8a08\u6578\u503c\u3002<\/p>\n<p><strong>\u96fb\u71b1\u8207\u8f3b\u5c04\u8ca0\u8f09\u3002<\/strong> \u52a0\u71b1\u58d3\u677f\u3001\u64e0\u51fa\u6a5f\u6a5f\u7b52\u3001\u5e36\u6709\u52a0\u71b1\u7b52\u7684\u9ede\u81a0\u95a5\u3001\u534a\u5c0e\u9ad4\u8154\u9ad4\u9580\u3002\u9019\u4e9b\u5728\u5bc6\u5c01\u8655\u904b\u884c\u65bc 180 \u5230 250 \u00b0C\uff0c\u5e7e\u4e4e\u6c92\u6709\u6d41\u9ad4\u51b7\u537b\u3002\u5931\u6548\u6a21\u5f0f\u662f\u4e7e\u6c27\u5316\uff1a\u786c\u5316\u8207\u9f9c\u88c2\u800c\u975e\u81a8\u8139\uff0c\u800c\u4e14\u7531\u65bc\u52a0\u71b1\u5668\u4e0d\u540c\u5fc3\uff0c\u74b0\u7684\u4e00\u5074\u5e38\u5e38\u51fa\u73fe\u71b1\u9ede\u3002<\/p>\n<p><strong>\u5f15\u64ce\u8207\u6392\u6c23\u3002<\/strong> \u6e26\u8f2a\u589e\u58d3\u5668\u4f9b\u6cb9\u3001EGR \u8ff4\u8def\u3001\u7dca\u9130\u6392\u6c23\u7684\u588a\u7247\u3002250 \u5230 300 \u00b0C \u7684\u5cf0\u503c\u662f\u6b63\u5e38\u7684\uff0c\u800c\u4e14\u5bc6\u5c01\u4ef6\u9762\u5c0d\u7684\u662f\u71b1\u5faa\u74b0\u800c\u975e\u7a69\u614b\u3002\u71b1\u5faa\u74b0\u6bd4\u7a69\u5b9a\u53d7\u71b1\u66f4\u5177\u7834\u58de\u6027\uff0c\u56e0\u70ba\u6bcf\u4e00\u6b21\u5faa\u74b0\u90fd\u6703\u628a\u5bc6\u5c01\u4ef6\u91cd\u65b0\u64e0\u5165\u9593\u9699\uff0c\u518d\u5728\u51b7\u614b\u4e0b\u91cd\u65b0\u58d3\u7e2e\u3002<\/p>\n<h2>\u7b2c\u4e00\u6b65\uff1a\u91cf\u6e2c\u4f60\u771f\u6b63\u9762\u5c0d\u7684\u6eab\u5ea6<\/h2>\n<p>\u6211\u5011\u8abf\u67e5\u7684\u5927\u591a\u6578\u9ad8\u6eab\u61c9\u7528\u5931\u6548\uff0c\u90fd\u59cb\u65bc RFQ \u88e1\u4e00\u500b\u932f\u8aa4\u7684\u6578\u5b57\u3002\u4e09\u500b\u7fd2\u6163\u53ef\u4ee5\u89e3\u6c7a\u9019\u500b\u554f\u984c\u3002<\/p>\n<p>\u628a\u71b1\u96fb\u5076\u653e\u5728\u5bc6\u5c01\u4ef6\u4e0a\uff0c\u800c\u4e0d\u662f\u5916\u6bbc\u4e0a\u3002\u5728\u7a69\u614b\u4e0b\uff0c\u88dd\u5728\u8ef8\u627f\u5ea7\u6216\u6c7d\u7f38\u84cb\u5916\u5074\u7684\u63a2\u91dd\u8b80\u6578\u6703\u6bd4\u5bc6\u5c01\u4ecb\u9762\u4f4e 40 \u5230 80 \u00b0C\uff0c\u56e0\u70ba\u71b1\u8def\u5f91\u6703\u5148\u7d93\u904e\u5bc6\u5c01\u4ef6\u3002<\/p>\n<p>\u8a18\u9304\u505c\u6a5f\u56de\u71b1\u5cf0\u503c\u3002\u7576\u6cf5\u3001\u58d3\u7e2e\u6a5f\u6216\u63db\u71b1\u5668\u505c\u6b62\u6642\uff0c\u51b7\u537b\u6db2\u548c\u88fd\u7a0b\u6d41\u4e5f\u96a8\u4e4b\u505c\u6b62\uff0c\u4f46\u91d1\u5c6c\u8cea\u91cf\u4ecd\u6301\u7e8c\u628a\u71b1\u91cf\u704c\u5165\u5bc6\u5c01\u4ef6\u3002\u6bd4\u904b\u884c\u6eab\u5ea6\u9ad8 30 \u5230 60 \u00b0C \u7684\u505c\u6a5f\u56de\u71b1\u6eab\u5ea6\u662f\u6b63\u5e38\u7684\uff0c\u800c\u4e14\u53ef\u80fd\u6301\u7e8c\u6578\u5c0f\u6642\u3002\u5982\u679c\u5bc6\u5c01\u4ef6\u904b\u884c\u6642\u662f 205 \u00b0C\uff0c\u6bcf\u6b21\u505c\u6a5f\u5f8c\u53c8\u6709\u5169\u5c0f\u6642\u8655\u65bc 250 \u00b0C\uff0c\u90a3\u9ebc\u6750\u6599\u5fc5\u9808\u80fd\u627f\u53d7 250 \u00b0C\uff0c\u800c\u4e0d\u662f 205 \u00b0C\u3002<\/p>\n<p>\u8a18\u9304\u555f\u52d5\u5347\u6eab\u66f2\u7dda\u3002\u4e00\u500b 25 \u00b0C \u7684\u5bc6\u5c01\u4ef6\u58d3\u5728\u56db\u5206\u9418\u5167\u5347\u5230 200 \u00b0C \u7684\u6cd5\u862d\u4e0a\uff0c\u6703\u770b\u5230\u6cd5\u862d\u5148\u81a8\u8139\u800c\u5bc6\u5c01\u4ef6\u9084\u6c92\u8ddf\u4e0a\u3002\u9019\u7a2e\u5dee\u7570\u6b63\u662f\u5543\u8755\u548c\u6e9d\u69fd\u78e8\u640d\u7684\u8d77\u9ede\u3002<\/p>\n<h2>\u56db\u500b\u7cfb\u5217\uff0c\u9644\u6578\u64da<\/h2>\n<p>\u4e0b\u8868\u7d66\u51fa\u5728\u4e7e\u7a7a\u6c23\u6216\u60f0\u6027\u6c23\u9ad4\u4e2d\u7684\u5be6\u7528\u9023\u7e8c\u6975\u9650\uff0c\u4ee5\u53ca\u77ed\u671f\u5cf0\u503c\u3002\u84b8\u6c7d\u3001\u9ad8\u82ef\u80fa\u9ede\u71b1\u6cb9\u3001\u80fa\u985e\u548c\u6c27\u5316\u5291\u90fd\u6703\u628a\u9019\u4e9b\u6578\u5b57\u62c9\u4f4e\u3002\u628a\u9023\u7e8c\u6b04\u7576\u4f5c\u8a2d\u8a08\u76ee\u6a19\uff0c\u628a\u5cf0\u503c\u6b04\u7576\u4f5c\u4f60\u80fd\u627f\u53d7\u5e7e\u6b21\u7684\u4e8b\u4ef6\uff0c\u800c\u4e0d\u662f\u4e00\u7a2e\u73ed\u6b21\u6a21\u5f0f\u3002<\/p>\n<table>\n<thead>\n<tr>\n<th>\u6750\u6599<\/th>\n<th>\u9023\u7e8c\u6700\u9ad8<\/th>\n<th>\u77ed\u671f\u5cf0\u503c<\/th>\n<th>\u6700\u4f4e\u6975\u9650<\/th>\n<th>\u5f48\u6027\u56de\u5fa9<\/th>\n<th>\u6210\u672c\u6307\u6578<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>HNBR<\/td>\n<td>150 \u00b0C<\/td>\n<td>175 \u00b0C<\/td>\n<td>-40 \u00b0C<\/td>\n<td>\u826f\u597d<\/td>\n<td>1.5\u00d7<\/td>\n<\/tr>\n<tr>\n<td>VMQ \u77fd\u81a0<\/td>\n<td>200 \u00b0C<\/td>\n<td>230 \u00b0C<\/td>\n<td>-60 \u00b0C<\/td>\n<td>\u826f\u597d\uff0c\u5f37\u5ea6\u4f4e<\/td>\n<td>2\u00d7<\/td>\n<\/tr>\n<tr>\n<td>FKM\uff08\u6a19\u6e96\uff09<\/td>\n<td>200 \u00b0C<\/td>\n<td>230 \u00b0C<\/td>\n<td>-20 \u00b0C<\/td>\n<td>\u826f\u597d<\/td>\n<td>3\u00d7<\/td>\n<\/tr>\n<tr>\n<td>FEPM\uff08AFLAS \u578b\uff09<\/td>\n<td>200 \u00b0C<\/td>\n<td>230 \u00b0C<\/td>\n<td>-5 \u00b0C<\/td>\n<td>\u826f\u597d<\/td>\n<td>6\u00d7<\/td>\n<\/tr>\n<tr>\n<td>\u6c1f\u6a61\u81a0<\/td>\n<td>260\u2013325 \u00b0C<\/td>\n<td>300\u2013350 \u00b0C<\/td>\n<td>-15 \u00b0C<\/td>\n<td>\u826f\u597d<\/td>\n<td>40\u201380\u00d7<\/td>\n<\/tr>\n<tr>\n<td>PTFE\uff0c\u7d14\u6599\u8207\u586b\u5145<\/td>\n<td>260 \u00b0C<\/td>\n<td>280 \u00b0C<\/td>\n<td>-200 \u00b0C<\/td>\n<td>\u7121\u5f48\u7c27\u5247\u4e0d\u9069\u7528<\/td>\n<td>1\u20131.5\u00d7<\/td>\n<\/tr>\n<tr>\n<td>\u7aba\u8996<\/td>\n<td>250 \u00b0C<\/td>\n<td>300 \u00b0C<\/td>\n<td>-60 \u00b0C<\/td>\n<td>\u7121<\/td>\n<td>8\u201312\u00d7<\/td>\n<\/tr>\n<tr>\n<td>\u67d4\u6027\u77f3\u58a8<\/td>\n<td>\u7a7a\u6c23\u4e2d 450 \u00b0C<\/td>\n<td>\u60f0\u6027\u6c23\u9ad4\u4e2d\u66f4\u9ad8<\/td>\n<td>-200 \u00b0C<\/td>\n<td>\u7121<\/td>\n<td>2\u00d7<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"note\">\u6210\u672c\u6307\u6578\u4ee5\u76f8\u540c\u5c3a\u5bf8\u7684\u6a19\u6e96 NBR O \u578b\u74b0\u70ba\u57fa\u6e96\uff0c\u6839\u64da\u6211\u5011\u81ea\u8eab\u7684\u91cf\u7522\u5831\u50f9\u8a18\u9304\u8a08\u7b97\u3002\u6b64\u70ba\u6578\u91cf\u7d1a\u53c3\u8003\uff0c\u4e26\u975e\u50f9\u76ee\u8868\u3002<\/p>\n<p>\u8acb\u5c07\u6b64\u8868\u8996\u70ba\u968e\u68af\uff0c\u800c\u975e\u83dc\u55ae\u3002\u6bcf\u4e00\u7d1a\u7d04\u53ef\u63db\u53d6 30 \u81f3 60 \u00b0C \u7684\u9023\u7e8c\u4f7f\u7528\u6eab\u5ea6\uff0c\u800c\u6210\u672c\u5247\u6bd4\u4e0b\u4e00\u7d1a\u9ad8\u51fa\u4e09\u81f3\u5341\u500d\u3002\u5de5\u7a0b\u4e0a\u7684\u554f\u984c\u5f9e\u4f86\u4e0d\u662f\u300c\u54ea\u7a2e\u6750\u6599\u6700\u597d\u300d\uff0c\u800c\u662f\u300c\u54ea\u7a2e\u6700\u4fbf\u5b9c\u7684\u6750\u6599\u80fd\u6490\u904e\u6574\u500b\u5de5\u4f5c\u5faa\u74b0\u300d\u3002<\/p>\n<h2>\u6c7a\u5b9a\u6027\u56e0\u7d20\u662f\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\uff0c\u800c\u975e\u6578\u64da\u8868\u6eab\u5ea6<\/h2>\n<p>\u6bcf\u4efd\u81a0\u6599\u6578\u64da\u8868\u90fd\u5217\u6709\u6eab\u5ea6\u7b49\u7d1a\u8207\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u6578\u503c\u3002\u8cb7\u5bb6\u53ea\u770b\u524d\u8005\uff0c\u5ffd\u7565\u5f8c\u8005\u3002\u800c\u5f8c\u8005\u624d\u662f\u9810\u6e2c\u6d29\u6f0f\u7684\u95dc\u9375\u3002<\/p>\n<p>\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u4f9d ASTM D395 \u65b9\u6cd5 B\uff08\u6216 ISO 815\uff09\u6e2c\u5b9a\uff1a\u5c07\u8a66\u6a23\u58d3\u7e2e 25%\uff0c\u5728\u6307\u5b9a\u6eab\u5ea6\u4e0b\u4fdd\u6301\u56fa\u5b9a\u6642\u9593\u2014\u2014\u5e38\u898b\u70ba 22 \u5c0f\u6642\u6216 70 \u5c0f\u6642\u2014\u2014\u91cb\u653e\u5f8c\u8b93\u5176\u6062\u5fa9 30 \u5206\u9418\uff0c\u518d\u9032\u884c\u91cf\u6e2c\u3002\u7d50\u679c\u5373\u70ba\u539f\u59cb\u8b8a\u5f62\u91cf\u4e2d\u672a\u80fd\u56de\u5fa9\u7684\u767e\u5206\u6bd4\u3002<\/p>\n<table>\n<thead>\n<tr>\n<th>\u6750\u6599<\/th>\n<th>150 \u00b0C \u4e0b 70 \u5c0f\u6642<\/th>\n<th>200 \u00b0C \u4e0b 70 \u5c0f\u6642<\/th>\n<th>230 \u00b0C \u4e0b 70 \u5c0f\u6642<\/th>\n<th>\u5099\u8a3b<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>NBR 70<\/td>\n<td>25\u201335%<\/td>\n<td>\u672a\u8a55\u7d1a<\/td>\n<td>\u2014<\/td>\n<td>\u8d85\u904e 120 \u00b0C \u6703\u5feb\u901f\u786c\u5316<\/td>\n<\/tr>\n<tr>\n<td>HNBR 70<\/td>\n<td>20\u201330%<\/td>\n<td>40\u201355%<\/td>\n<td>\u2014<\/td>\n<td>\u904e\u6c27\u5316\u7269\u786b\u5316\u7b49\u7d1a\u7dad\u6301\u66f4\u4e45<\/td>\n<\/tr>\n<tr>\n<td>FKM 75\uff0c\u96d9\u915a\u786b\u5316<\/td>\n<td>15\u201325%<\/td>\n<td>30\u201345%<\/td>\n<td>45\u201360%<\/td>\n<td>\u6a19\u6e96\u4e3b\u529b\u6750\u6599<\/td>\n<\/tr>\n<tr>\n<td>FKM 75\uff0c\u904e\u6c27\u5316\u7269\u786b\u5316<\/td>\n<td>12\u201320%<\/td>\n<td>25\u201335%<\/td>\n<td>35\u201350%<\/td>\n<td>\u5728\u84b8\u6c7d\u53ca\u9e7c\u6027\u74b0\u5883\u4e2d\u8868\u73fe\u66f4\u4f73<\/td>\n<\/tr>\n<tr>\n<td>FFKM 75<\/td>\n<td>10\u201318%<\/td>\n<td>15\u201325%<\/td>\n<td>20\u201335%<\/td>\n<td>\u8996\u7b49\u7d1a\u800c\u5b9a\uff0c\u8acb\u67e5\u6838\u5831\u544a<\/td>\n<\/tr>\n<tr>\n<td>VMQ 70<\/td>\n<td>15\u201325%<\/td>\n<td>25\u201340%<\/td>\n<td>40\u201360%<\/td>\n<td>\u5f37\u5ea6\u4f4e\u9650\u5236\u5176\u7528\u9014<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p class=\"note\">\u4ee5\u4e0a\u7bc4\u570d\u5f59\u7de8\u81ea\u5df2\u767c\u4f48\u7684\u81a0\u6599\u6578\u64da\u8868\u3002\u8acb\u5411\u4f9b\u61c9\u5546\u7d22\u53d6\u5be6\u969b\u6279\u6b21\u7684\u6e2c\u8a66\u5831\u544a\uff0c\u800c\u975e\u7cfb\u5217\u5178\u578b\u503c\u3002\u6b64\u8868\u4e0a 10 \u9ede\u7684\u5dee\u8ddd\uff0c\u5c31\u662f\u5169\u5e74\u5bc6\u5c01\u58fd\u547d\u8207\u516d\u500b\u6708\u5bc6\u5c01\u58fd\u547d\u4e4b\u9593\u7684\u5dee\u5225\u3002<\/p>\n<p>\u7531\u6b64\u5f97\u51fa\u5169\u689d\u898f\u5247\u3002\u7b2c\u4e00\uff0c\u82e5\u61c9\u7528\u9577\u671f\u8655\u65bc 200 \u00b0C\uff0c\u6a19\u6e96 FKM \u5728\u8a72\u6eab\u5ea6\u4e0b\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u9054 35%\uff0c\u5176\u5bc6\u5c01\u4ef6\u6703\u5728\u4e00\u81f3\u5169\u5e74\u5167\u9010\u6f38\u8815\u8b8a\u81f3\u5931\u6548\uff1b\u904e\u6c27\u5316\u7269\u786b\u5316\u7b49\u7d1a\u6216 FFKM \u5247\u53ef\u591a\u7528\u6578\u5e74\u3002\u7b2c\u4e8c\uff0c\u82e5\u61c9\u7528\u5728\u5176\u904b\u884c\u6642\u9593\u7684 10% \u5167\u9054\u5230 230 \u00b0C\uff0c\u771f\u6b63\u95dc\u9375\u7684\u8001\u5316\u5c31\u767c\u751f\u5728\u90a3 10% \u671f\u9593\uff0c\u4e14\u4ee5\u52a0\u901f\u901f\u7387\u9032\u884c\u2014\u2014\u6bcf\u8d85\u51fa\u984d\u5b9a\u9023\u7e8c\u4e0a\u9650 10 \u00b0C\uff0c\u8001\u5316\u901f\u7387\u7d04\u52a0\u500d\u3002<\/p>\n<h2>200 \u00b0C \u4e0b\u7684 FKM\uff1a\u8a72\u9078\u54ea\u500b\u7b49\u7d1a\uff0c\u6975\u9650\u5728\u54ea\u88e1<\/h2>\n<p>\u6a19\u6e96 FKM\u2014\u2014\u5373\u4f54\u5e02\u5834\u5927\u90e8\u5206\u7684 A \u578b\u96d9\u915a\u786b\u5316\u81a0\u6599\u2014\u2014\u662f\u4e7e\u71e5\u7a7a\u6c23\u3001\u6db2\u58d3\u6cb9\u3001\u67f4\u6cb9\u3001\u6f64\u6ed1\u8102\u53ca\u5927\u591a\u6578\u7926\u7269\u6cb9\u5728 200 \u00b0C \u9023\u7e8c\u4f7f\u7528\u4e0b\u7684\u6b63\u78ba\u9078\u64c7\u3002\u4f46\u5728\u4ee5\u4e0b\u4e09\u7a2e\u7d93\u5e38\u51fa\u73fe\u7684\u60c5\u6cc1\u4e0b\uff0c\u5b83\u5c31\u662f\u932f\u8aa4\u7684\u9078\u64c7\uff1a<\/p>\n<ul>\n<li><strong>150 \u00b0C \u4ee5\u4e0a\u7684\u84b8\u6c7d\u53ca\u71b1\u6c34\u3002<\/strong> \u6703\u767c\u751f\u812b\u6c1f\u5316\u6c2b\u53cd\u61c9\u3002\u908a\u7de3\u60c5\u6cc1\u53ef\u6539\u7528\u904e\u6c27\u5316\u7269\u786b\u5316 FKM\uff0c\u771f\u6b63\u9700\u8981\u84b8\u6c7d\u670d\u52d9\u5247\u7528 FEPM\uff08AFLAS \u578b\uff09\u6216 EPDM\u3002<\/li>\n<li><strong>\u80fa\u985e\u3001\u6c28\u53ca\u591a\u7a2e\u9e7c\u6027\u6e05\u6f54\u5291\u3002<\/strong> FKM \u6703\u81a8\u8139\u4e26\u8edf\u5316\u3002\u61c9\u6539\u7528 FFKM \u6216 PTFE\u3002<\/li>\n<li><strong>-20 \u00b0C \u4ee5\u4e0b\u51b7\u555f\u52d5\uff0c\u540c\u6642\u9700\u627f\u53d7 200 \u00b0C \u4f7f\u7528\u6eab\u5ea6\u3002<\/strong> \u6a19\u6e96 FKM \u7684\u73bb\u7483\u5316\u8f49\u8b8a\u6eab\u5ea6\u7d04\u70ba -18 \u81f3 -20 \u00b0C\uff0c\u51b7\u555f\u52d5\u6642\u6703\u9f9c\u88c2\u3002\u4f4e\u6eab\u7b49\u7d1a\u53ef\u5c07\u6b64\u4e0b\u9650\u5ef6\u4f38\u81f3\u7d04 -40 \u00b0C\uff0c\u4f46\u901a\u5e38\u6703\u72a7\u7272\u90e8\u5206\u9ad8\u6eab\u6297\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u80fd\u529b\u3002<\/li>\n<\/ul>\n<p>\u5728\u4efb\u4f55\u540c\u6642\u63a5\u89f8\u6c34\u3001\u51b7\u537b\u6db2\u6216 CIP \u5316\u5b78\u54c1\u7684\u71b1\u61c9\u7528\u4e2d\uff0c\u904e\u6c27\u5316\u7269\u786b\u5316 FKM \u503c\u5f97\u591a\u4ed8 10 \u81f3 20% \u7684\u6ea2\u50f9\u3002\u96d9\u915a\u786b\u5316\u6703\u53d7\u8a31\u591a\u9e7c\u6027\u6e05\u6d17\u5faa\u74b0\u4e2d\u7684\u9e7c\u4fb5\u8755\uff0c\u904e\u6c27\u5316\u7269\u786b\u5316\u5247\u4e0d\u6703\u3002\u82e5\u60a8\u7684\u7522\u7dda\u6bcf\u665a\u4ee5 80 \u00b0C \u82db\u6027\u9e7c\u6e05\u6d17\uff0c\u6c7a\u5b9a\u5bc6\u5c01\u58fd\u547d\u7684\u5c31\u662f\u9019\u500b\u5dee\u7570\uff0c\u800c\u975e 200 \u00b0C \u7684\u984d\u5b9a\u503c\u3002<\/p>\n<h2>FFKM\uff1a\u984d\u5916 60 \u00b0C \u7684\u4ee3\u50f9<\/h2>\n<p>\u5168\u6c1f\u6a61\u81a0\u4ee5\u6c1f\u53d6\u4ee3\u805a\u5408\u7269\u4e3b\u93c8\u4e0a\u7684\u6bcf\u4e00\u500b\u6c2b\u539f\u5b50\u3002\u50c5\u6b64\u4e00\u9805\u6539\u8b8a\uff0c\u5373\u53ef\u5c07\u9023\u7e8c\u4f7f\u7528\u6eab\u5ea6\u63a8\u5347\u81f3 260\u2013325 \u00b0C\uff08\u8996\u7b49\u7d1a\u800c\u5b9a\uff09\uff0c\u4e26\u4f7f\u8a72\u6750\u6599\u5e7e\u4e4e\u80fd\u62b5\u6297\u4e00\u5207\uff0c\u9664\u4e86\u9ad8\u6eab\u4e0b\u7684\u7194\u878d\u9e7c\u91d1\u5c6c\u53ca\u5143\u7d20\u6c1f\u3002<\/p>\n<p>\u5b83\u540c\u6642\u6539\u8b8a\u4e86\u8a2d\u8a08\u898f\u5247\u3002FFKM \u7684\u6297\u62c9\u5f37\u5ea6\u53ca\u6297\u6495\u88c2\u6027\u5747\u4f4e\u65bc FKM\uff0c\u56e0\u6b64\u5c0d\u5c16\u92b3\u6e9d\u69fd\u908a\u7de3\u7684\u5bb9\u5fcd\u5ea6\u8f03\u4f4e\uff0c\u5b89\u88dd\u6642\u4e5f\u66f4\u5bb9\u6613\u88ab\u5543\u50b7\u3002\u5176\u71b1\u81a8\u8139\u4fc2\u6578\u8f03\u9ad8\uff0c\u5728\u5927\u76f4\u5f91\u61c9\u7528\u4e0a\u5c24\u70ba\u91cd\u8981\u3002\u800c\u5728\u9ad8\u58d3\u6c23\u9ad4\u670d\u52d9\u4e2d\u2014\u2014\u6c2b\u6c23\u3001\u6c2e\u6c23\u3001CO2\u3001\u5929\u7136\u6c23\u2014\u2014\u5b83\u6613\u53d7\u5feb\u901f\u6c23\u9ad4\u6e1b\u58d3\u640d\u50b7\uff1a\u6c23\u9ad4\u5728\u58d3\u529b\u4e0b\u6eb6\u5165\u805a\u5408\u7269\uff0c\u58d3\u529b\u9a5f\u964d\u6642\u6025\u5287\u81a8\u8139\uff0c\u5f9e\u5167\u90e8\u4f7f\u5bc6\u5c01\u4ef6\u8d77\u6ce1\u3002\u89e3\u6c7a\u65b9\u6848\u662f\u63a1\u7528\u786c\u5ea6 90 Shore A \u4e14\u5177\u660e\u78ba\u964d\u58d3\u901f\u7387\u7684\u6297\u6e1b\u58d3\u7b49\u7d1a\uff0c\u800c\u975e\u6a19\u6e96 FFKM \u74b0\u3002<\/p>\n<p>FFKM \u6210\u672c\u70ba NBR \u7684 40 \u81f3 80 \u500d\uff0c\u50c5\u5728\u4ee5\u4e0b\u4e09\u7a2e\u60c5\u6cc1\u4e0b\u624d\u503c\u5f97\u63a1\u7528\uff1a\u6eab\u5ea6\u6301\u7e8c\u9ad8\u65bc 230 \u00b0C\uff1b\u5316\u5b78\u74b0\u5883\u6703\u7834\u58de FKM\uff08\u80fa\u985e\u3001\u5f37\u9e7c\u3001\u916e\u985e\u3001\u71b1\u9178\uff09\uff1b\u6216\u5bc6\u5c01\u4ef6\u96e3\u4ee5\u89f8\u53ca\uff0c\u505c\u6a5f\u6210\u672c\u9060\u8d85\u96f6\u4ef6\u6210\u672c\u3002\u82e5\u4e09\u8005\u7686\u4e0d\u6210\u7acb\uff0cFFKM \u53ea\u662f\u63a9\u84cb\u8a2d\u8a08\u554f\u984c\u7684\u6602\u8cb4\u65b9\u5f0f\u3002<\/p>\n<figure><img loading=\"lazy\" decoding=\"async\" src=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2026\/11\/a1_aged.jpg\" alt=\"\u5728 200 \u00b0C \u7a7a\u6c23\u5faa\u74b0\u70d8\u7bb1\u4e2d\u653e\u7f6e 70 \u5c0f\u6642\u5f8c\uff0c\u8001\u5316 FKM O \u578b\u74b0\u8207\u65b0 O \u578b\u74b0\u4e26\u5217\" width=\"1536\" height=\"1024\" \/><figcaption>\u5de6\u5716\uff1aFKM \u65bc 200 \u00b0C \u4e0b\u7d93 70 \u5c0f\u6642\u5f8c\u3002\u622a\u9762\u5df2\u58d3\u6241\u3001\u8868\u9762\u5df2\u786c\u5316\u2014\u2014\u7d42\u7d50\u5bc6\u5c01\u58fd\u547d\u7684\u662f\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\uff0c\u800c\u975e\u7194\u5316\u3002<\/figcaption><\/figure>\n<h2>PTFE \u8207 PEEK\uff1a\u7121\u5f48\u6027\u56de\u5fa9\uff0c\u6545\u9808\u64da\u6b64\u8a2d\u8a08<\/h2>\n<p>\u5169\u7a2e\u6750\u6599\u7686\u80fd\u5728 250\u2013260 \u00b0C \u4e0b\u4fdd\u6301\u5176\u7279\u6027\uff0c\u4e26\u5e7e\u4e4e\u62b5\u6297\u6240\u6709\u6d41\u9ad4\u3002\u4f46\u5169\u8005\u90fd\u4e0d\u50cf\u6a61\u81a0\u3002PTFE \u5728\u8ca0\u8f09\u4e0b\u6703\u8815\u8b8a\uff0c\u4e14\u57fa\u672c\u4e0a\u6c92\u6709\u5f48\u6027\u8a18\u61b6\uff0c\u56e0\u6b64\u6e9d\u69fd\u4e2d\u7684\u7d14 PTFE \u74b0\u4e00\u65e6\u58d3\u529b\u4e0b\u964d\u5c31\u6703\u6d29\u6f0f\u3002\u6a19\u6e96\u89e3\u6c7a\u65b9\u6848\u662f\u5f48\u7c27\u84c4\u80fd\u8a2d\u8a08\uff1a\u5728 PTFE \u5916\u5957\u5167\u7f6e\u5165\u659c\u5708\u3001\u87ba\u65cb\u6216\u61f8\u81c2\u5f48\u7c27\uff0c\u63d0\u4f9b\u805a\u5408\u7269\u672c\u8eab\u7121\u6cd5\u7522\u751f\u7684\u6c38\u4e45\u8ca0\u8f09\u3002<\/p>\n<p>PEEK \u70ba\u6a5f\u68b0\u52a0\u5de5\u800c\u975e\u6a21\u5851\u6210\u578b\uff0c\u56e0\u6b64\u975e\u5e38\u9069\u5408\u7528\u65bc 250 \u00b0C \u4e0b\u5f48\u6027\u9ad4\u6703\u64e0\u51fa\u7684\u5099\u7528\u74b0\u3001\u5c0e\u5411\u5143\u4ef6\u3001\u71c8\u7c60\u74b0\u53ca\u8010\u78e8\u96f6\u4ef6\u3002\u5b83\u4ea6\u7528\u4f5c\u9ad8\u6eab\u6b62\u56de\u95a5\u7684\u95a5\u5ea7\u6750\u6599\u3002\u5b83\u505a\u4e0d\u5230\u7684\u662f\u5728\u4f4e\u58d3\u4e0b\u81ea\u884c\u52d5\u614b\u5bc6\u5c01\u2014\u2014\u5b83\u6c92\u6709\u56de\u5fa9\u80fd\u529b\uff0c\u56e0\u6b64\u63a5\u89f8\u58d3\u529b\u5fc5\u9808\u4f86\u81ea\u5176\u4ed6\u4f86\u6e90\u3002<\/p>\n<p>\u5728 200 \u00b0C \u4ee5\u4e0a\uff0c\u6211\u5011\u6700\u5e38\u51fa\u8ca8\u7684\u7d44\u5408\u662f FKM \u6216 FFKM O \u578b\u74b0\uff0c\u5169\u5074\u914d\u4ee5 PEEK \u5099\u7528\u74b0\u3002\u5f48\u6027\u9ad4\u63d0\u4f9b\u5bc6\u5c01\uff1bPEEK \u5247\u9632\u6b62\u8edf\u5316\u7684\u5f48\u6027\u9ad4\u64e0\u5165\u9593\u9699\u3002\u5728 200 \u00b0C \u53ca 20 MPa \u4e0b\uff0c\u7121\u5099\u7528\u74b0\u7684 75 Shore A \u74b0\u6703\u5728\u6578\u5c0f\u6642\u5167\u56e0\u64e0\u51fa\u800c\u5931\u6548\u3002\u6211\u5011\u7684 <a href=\"https:\/\/www.bosssealing.com\/zh\/%e7%94%a2%e5%93%81%e5%88%86%e9%a1%9e\/%e5%a2%8a%e7%89%87%e8%8f%af%e5%8f%b8-%e6%94%af%e6%92%90%e7%92%b0\/\">\u5099\u7528\u74b0\u7cfb\u5217<\/a> \u6db5\u84cb\u6a19\u6e96\u622a\u9762\u5c3a\u5bf8\u7684 PEEK\u3001\u586b\u5145 PTFE \u53ca POM\uff0c\u4ee5\u53ca <a href=\"https:\/\/www.bosssealing.com\/zh\/%e7%94%a2%e5%93%81%e5%88%86%e9%a1%9e\/%e5%bd%88%e7%b0%a7%e8%93%84%e8%83%bd%e5%af%86%e5%b0%81%e5%9c%88-%e8%ae%8a%e9%ab%94%e5%af%86%e5%b0%81\/\">\u5f48\u7c27\u84c4\u80fd\u7cfb\u5217<\/a> \u6db5\u84cb PTFE \u8b77\u5957\u9808\u81ea\u884c\u627f\u64d4\u5bc6\u5c01\u529f\u80fd\u7684\u60c5\u6cc1\u3002<\/p>\n<h2>300 \u00b0C \u4ee5\u4e0a\uff1a\u77f3\u58a8\u3001\u91d1\u5c6c\u53ca\u9676\u74f7<\/h2>\n<p>\u4e00\u65e6\u9700\u6c42\u8d85\u904e 300 \u00b0C\uff0c\u5f48\u6027\u9ad4\u4fbf\u4e0d\u518d\u9069\u7528\u3002\u67d4\u6027\u77f3\u58a8\u586b\u6599\u53ca\u588a\u7247\u5728\u7a7a\u6c23\u4e2d\u53ef\u627f\u53d7 450 \u00b0C\uff0c\u5728\u60f0\u6027\u6c23\u9ad4\u4e2d\u6216\u53d7\u58d3\u72c0\u614b\u4e0b\u66f4\u80fd\u627f\u53d7\u9060\u9ad8\u65bc\u6b64\u7684\u6eab\u5ea6\uff0c\u662f\u95a5\u687f\u586b\u6599\u53ca\u9ad8\u6eab\u6cd5\u862d\u7684\u6a19\u6e96\u65b9\u6848\u3002\u7576\u58d3\u529b\u3001\u71b1\u5faa\u74b0\u53ca\u6ef2\u900f\u540c\u6642\u69cb\u6210\u95dc\u9375\u56e0\u7d20\u6642\uff0c\u5247\u7531 316L\u3001Inconel \u6216 Monel \u88fd\u6210\u7684\u91d1\u5c6c C \u5f62\u74b0\u3001O \u5f62\u74b0\u53ca E \u5f62\u74b0\u63a5\u624b\u3002<\/p>\n<p>\u9019\u4e9b\u5bc6\u5c01\u4ef6\u5c07\u96e3\u9ede\u5f9e\u6750\u6599\u8f49\u79fb\u5230\u786c\u4ef6\u3002\u91d1\u5c6c\u5bc6\u5c01\u4ef6\u9700\u8981\u9ad8\u800c\u7a69\u5b9a\u7684\u87ba\u6813\u8f09\u8377\u3001\u975e\u5e38\u5e73\u6574\u7684\u6cd5\u862d\uff0c\u4ee5\u53ca\u9054 Ra 0.4 \u00b5m \u6216\u66f4\u4f73\u7684\u8868\u9762\u5149\u6f54\u5ea6\u3002\u9664\u975e\u6cd5\u862d\u8207\u87ba\u6813\u6750\u6599\u4e92\u76f8\u5339\u914d\uff0c\u5426\u5247\u5b83\u5011\u96e3\u4ee5\u627f\u53d7\u71b1\u5faa\u74b0\uff0c\u4e26\u4e14\u9700\u8981\u660e\u78ba\u7684\u58d3\u6f70\u6216\u56de\u5f48\u9918\u91cf\u3002\u77f3\u58a8\u5247\u9700\u8981\u4fdd\u6301\u58d3\u7e2e\u91cf\u53ca\u6297\u6c27\u5316\u4fdd\u8b77\uff1b\u5728 450 \u00b0C \u4ee5\u4e0a\u7684\u6c27\u5316\u6027\u6c23\u6c1b\u4e2d\uff0c\u5b83\u6703\u76f4\u63a5\u71d2\u5931\u3002<\/p>\n<h2>\u9ad8\u6eab\u63a5\u982d\u7684\u786c\u4ef6\u898f\u5247<\/h2>\n<p>\u6211\u5011\u898b\u5230\u7684\u9ad8\u6eab\u5931\u6548\u500b\u6848\u4e2d\uff0c\u6709\u4e00\u534a\u5176\u5be6\u662f\u62ab\u7740\u6750\u6599\u5916\u8863\u7684\u786c\u4ef6\u554f\u984c\u3002\u4ee5\u4e0b\u56db\u689d\u898f\u5247\u6db5\u84cb\u4e86\u5927\u90e8\u5206\u60c5\u6cc1\u3002<\/p>\n<table>\n<thead>\n<tr>\n<th>\u53c3\u6578<\/th>\n<th>200 \u00b0C \u4e0b\u7684\u898f\u5247<\/th>\n<th>\u70ba\u4f55\u91cd\u8981<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>\u64e0\u51fa\u9593\u9699<\/td>\n<td>75 Shore A \u7121\u64cb\u5708\u6642\u6700\u5927 0.15 mm\uff1b\u914d PEEK \u64cb\u5708\u6642 0.25 mm<\/td>\n<td>\u9ad8\u6eab\u4e0b\u7684\u6a21\u91cf\u7d04\u70ba\u5ba4\u6eab\u503c\u7684\u4e00\u534a<\/td>\n<\/tr>\n<tr>\n<td>\u6e9d\u69fd\u8868\u9762\u5149\u6f54\u5ea6<\/td>\n<td>\u5bc6\u5c01\u9762\u9054 Ra 0.8 \u00b5m \u6216\u66f4\u4f73\uff1b\u4e0d\u5f97\u6709\u8ef8\u5411\u522e\u75d5<\/td>\n<td>\u53d7\u71b1\u7684\u6a61\u81a0\u8f03\u8edf\uff0c\u6703\u9806\u61c9\u522e\u75d5\u8b8a\u5f62\uff0c\u7136\u5f8c\u5728\u91cb\u653e\u6642\u6495\u88c2<\/td>\n<\/tr>\n<tr>\n<td>\u6e9d\u69fd\u586b\u5145\u7387<\/td>\n<td>\u4fdd\u6301 O \u5f62\u74b0\u622a\u9762\u9762\u7a4d\u4f4e\u65bc\u6e9d\u69fd\u9762\u7a4d\u7684 85%<\/td>\n<td>\u586b\u5145\u7387\u66f4\u9ad8\u6642\uff0c\u5f48\u6027\u9ad4\u7684\u71b1\u81a8\u8139\u7121\u8655\u53ef\u53bb<\/td>\n<\/tr>\n<tr>\n<td>\u6cd5\u862d\u53ca\u87ba\u6813\u6750\u6599<\/td>\n<td>\u81a8\u8139\u7cfb\u6578\u5339\u914d\u8aa4\u5dee\u7d04\u5728 15% \u4ee5\u5167<\/td>\n<td>200 \u00b0C \u4e0b\u7684\u5dee\u7570\u81a8\u8139\u6703\u4ee4\u63a5\u982d\u5f35\u958b\u7684\u901f\u5ea6\u5feb\u65bc\u5bc6\u5c01\u4ef6\u6240\u80fd\u8ddf\u96a8<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u518d\u52a0\u5169\u689d\u5b89\u88dd\u898f\u5247\u3002\u5728 150 \u00b0C \u4ee5\u4e0a\u88dd\u914d\u6642\uff0c\u52a0\u71b1\u5bc6\u5c01\u4ef6\u800c\u975e\u6e9d\u69fd\u2014\u2014\u6eab\u6696\u7684\u5bc6\u5c01\u4ef6\u66f4\u9806\u670d\uff0c\u4ea6\u8f03\u4e0d\u6613\u88ab\u6e9d\u69fd\u908a\u7de3\u5272\u50b7\u3002\u53e6\u5916\uff0c\u5207\u52ff\u91cd\u7528\u66fe\u7d93\u8655\u65bc\u9ad8\u6eab\u7684\u5bc6\u5c01\u4ef6\uff1a\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u662f\u4e0d\u53ef\u9006\u7684\uff0c\u7528\u904e\u7684\u5bc6\u5c01\u74b0\u5df2\u8017\u6389\u5176\u90e8\u5206\u58fd\u547d\u3002<\/p>\n<h2>\u7d93\u5f97\u8d77\u5be9\u6838\u7684\u9078\u578b\u6d41\u7a0b<\/h2>\n<p>\u9019\u662f\u6211\u5011\u8655\u7406\u9ad8\u6eab\u61c9\u7528\u4f86\u6599\u8a62\u50f9\u6642\u6240\u63a1\u7528\u7684\u6d41\u7a0b\u3002\u82e5\u5ba2\u6236\u5099\u6709\u6578\u64da\uff0c\u7d04\u9700 30 \u5206\u9418\uff0c\u4e26\u53ef\u907f\u514d\u5927\u90e8\u5206\u4ee3\u50f9\u9ad8\u6602\u7684\u932f\u8aa4\u3002<\/p>\n<ol>\n<li><strong>\u78ba\u5b9a\u6eab\u5ea6\u4e09\u8981\u7d20\u3002<\/strong> \u9023\u7e8c\u3001\u5cf0\u503c\u53ca\u6d78\u6ce1\u56de\u6eab\uff0c\u5404\u9644\u6301\u7e8c\u6642\u9593\u3002\u628a\u5b83\u5011\u5beb\u5728\u5716\u7d19\u4e0a\uff0c\u800c\u975e\u96fb\u90f5\u4e2d\u3002<\/li>\n<li><strong>\u8b58\u5225\u5bc6\u5c01\u4ef6\u8655\u7684\u6d41\u9ad4\uff0c\u800c\u975e\u5132\u7f50\u4e2d\u7684\u6d41\u9ad4\u3002<\/strong> \u6dfb\u52a0\u5291\u3001\u542b\u6c34\u91cf\u53ca\u5145\u6c23\u7a0b\u5ea6\u6703\u6539\u8b8a\u76f8\u5bb9\u6027\u3002\u542b 0.5% \u6c34\u5206\u7684\u71b1\u6cb9\u8207\u4e7e\u6cb9\u662f\u622a\u7136\u4e0d\u540c\u7684\u74b0\u5883\u3002<\/li>\n<li><strong>\u8a2d\u5b9a\u58d3\u529b\u53ca\u9593\u9699\u3002<\/strong> \u8a08\u7b97\u64cd\u4f5c\u6eab\u5ea6\u4e0b\u7684\u6700\u5927\u64e0\u51fa\u9593\u9699\uff0c\u5305\u62ec\u516c\u5dee\u758a\u52a0\u53ca\u71b1\u81a8\u8139\u3002<\/li>\n<li><strong>\u9078\u64c7\u80fd\u901a\u904e\u5168\u90e8\u4e09\u9805\u7684\u6700\u4f4e\u4e00\u7d1a\u3002<\/strong> \u7531 FKM \u958b\u59cb\uff0c\u50c5\u5728\u6eab\u5ea6\u9ad8\u65bc 230 \u00b0C \u6216\u5316\u5b78\u6027\u8cea\u6392\u9664 FKM \u6642\u624d\u6539\u7528 FFKM\u3002<\/li>\n<li><strong>\u52a0\u88dd\u64cb\u5708\u6216\u5c0e\u5411\u5143\u4ef6<\/strong> \u82e5\u9593\u9699\u8a08\u7b97\u7d50\u679c\u63a5\u8fd1\u81e8\u754c\u3001\u58d3\u529b\u8d85\u904e 20 MPa\uff0c\u6216\u5bc6\u5c01\u4ef6\u5c6c\u52d5\u614b\u61c9\u7528\u3002<\/li>\n<li><strong>\u754c\u5b9a\u9a57\u6536\u6e2c\u8a66\u3002<\/strong> \u9023\u7e8c\u6eab\u5ea6\u4e0b 70 \u5c0f\u6642\u5f8c\u7684\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u3001\u786c\u5ea6\u8b8a\u5316\uff0c\u4ee5\u53ca 24 \u5c0f\u6642\u6d41\u9ad4\u6d78\u6ce1\u4e26\u8a18\u9304\u9ad4\u7a4d\u81a8\u8139\u3002\u628a\u9650\u503c\u5beb\u5165\u63a1\u8cfc\u8a02\u55ae\u3002<\/li>\n<li><strong>\u7d22\u53d6\u6279\u6b21\u5831\u544a\u3002<\/strong> \u81a0\u6599\u6279\u6b21\u3001\u786b\u5316\u65e5\u671f\u3001\u5f8c\u786b\u5316\u9031\u671f\u53ca\u6e2c\u8a66\u6578\u64da\u3002\u6c92\u6709\u9019\u4e9b\uff0c\u4f60\u7121\u6cd5\u5206\u8fa8\u597d\u6279\u6b21\u8207\u50e5\u5016\u6279\u6b21\u3002<\/li>\n<\/ol>\n<h2>\u6211\u5011\u5728\u751f\u7522\u73fe\u5834\u6240\u898b<\/h2>\n<p>\u6211\u5011\u7684\u70d8\u7bb1\u70ba\u5ba2\u6236\u6279\u6b21\u9032\u884c 200 \u00b0C \u53ca 230 \u00b0C \u7684\u7a7a\u6c23\u5faa\u74b0\u8001\u5316\u6e2c\u8a66\uff0c\u6a21\u5f0f\u76f8\u7576\u4e00\u81f4\uff1a\u63d0\u65e9\u5931\u6548\u7684\u96f6\u4ef6\u5e7e\u4e4e\u5f9e\u4e0d\u662f\u805a\u5408\u7269\u9078\u932f\u7684\u90a3\u4e9b\uff0c\u800c\u662f\u70ba\u8d95\u8239\u671f\u800c\u7e2e\u77ed\u5f8c\u786b\u5316\u7684\u90a3\u4e9b\u3002\u5f8c\u786b\u5316\u2014\u2014\u5373\u9a45\u9664\u63ee\u767c\u7269\u4e26\u5b8c\u6210\u4ea4\u806f\u7684\u7b2c\u4e8c\u6b21\u70d8\u70e4\u2014\u2014\u6b63\u662f\u4ee4 FKM \u96f6\u4ef6\u4fdd\u6301 30% \u800c\u975e 50% \u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u7684\u95dc\u9375\u3002\u70ba\u7bc0\u7701\u4e00\u5929\u4ea4\u8ca8\u671f\u800c\u7701\u6389\u56db\u5c0f\u6642\u5f8c\u786b\u5316\uff0c\u4ee3\u50f9\u662f\u5ba2\u6236\u4e00\u5e74\u7684\u4f7f\u7528\u58fd\u547d\u3002<\/p>\n<p>\u7b2c\u4e8c\u500b\u6a21\u5f0f\u662f\u5c3a\u5bf8\u3002\u9ad8\u6eab\u5bc6\u5c01\u4ef6\u5728 23 \u00b0C \u4e0b\u6a19\u5b9a\uff0c\u537b\u5728 200 \u00b0C \u4e0b\u5b89\u88dd\uff0c\u800c\u5716\u7d19\u5f80\u5f80\u53ea\u8f09\u6709\u5ba4\u6eab\u516c\u5dee\u3002\u61c9\u7d22\u53d6\u76f4\u5f91\u4e0a\u7684\u71b1\u81a8\u8139\u9918\u91cf\u3002\u5c0d\u65bc 200 mm \u7684\u5bc6\u5c01\u74b0\uff0cFKM \u5728 23 \u00b0C \u81f3 200 \u00b0C \u4e4b\u9593\u7684\u81ea\u7531\u76f4\u5f91\u6703\u589e\u9577\u6578\u6beb\u7c73\u2014\u2014\u6bd4\u5468\u570d\u7684\u92fc\u6750\u9ad8\u51fa\u4e00\u500b\u6578\u91cf\u7d1a\u2014\u2014\u82e5\u6e9d\u69fd\u6c92\u6709\u5bb9\u7d0d\u8a72\u589e\u9577\u7684\u7a7a\u9593\uff0c\u5bc6\u5c01\u4ef6\u4e0d\u662f\u5c48\u66f2\u5c31\u662f\u64e0\u51fa\u3002<\/p>\n<p>\u7b2c\u4e09\u500b\u662f\u6587\u4ef6\u8a18\u9304\u3002\u5c0d\u65bc\u9ad8\u6eab\u5de5\u6cc1\uff0c\u8cb7\u5bb6\u61c9\u5805\u6301\u96a8\u8ca8\u9644\u4e0a\u81a0\u6599\u6279\u6b21\u8a18\u9304\u53ca\u8001\u5316\u6e2c\u8a66\u5831\u544a\u3002\u9019\u5728\u5de5\u5ee0\u7aef\u6beb\u7121\u6210\u672c\uff0c\u537b\u80fd\u5728\u5169\u5e74\u5f8c\u65bc\u5ee0\u623f\u89e3\u6c7a\u722d\u8b70\u3002<\/p>\n<h2>\u7d50\u8ad6<\/h2>\n<p>200 \u00b0C \u4ee5\u4e0a\uff0c\u6750\u6599\u9078\u64c7\u8fc5\u901f\u6536\u7a84\uff1aFKM \u5728\u4e7e\u6cb9\u6216\u7a7a\u6c23\u4e2d\u53ef\u9023\u7e8c\u627f\u53d7\u81f3 200 \u00b0C\uff0cFFKM \u9069\u7528\u65bc 230 \u00b0C \u4ee5\u4e0a\u6216\u5316\u5b78\u6027\u8cea\u4fb5\u8755 FKM \u7684\u5834\u5408\uff0c\u800c\u4e00\u65e6\u6eab\u5ea6\u8d85\u904e 260 \u00b0C \u6216\u6d41\u9ad4\u64ca\u6557\u6240\u6709\u5f48\u6027\u9ad4\uff0c\u5247\u6539\u7528 PTFE\u3001PEEK\u3001\u77f3\u58a8\u6216\u91d1\u5c6c\u3002\u9019\u90e8\u5206\u5f88\u7c21\u55ae\u3002<\/p>\n<p>\u6c7a\u5b9a\u5bc6\u5c01\u4ef6\u80fd\u5426\u6301\u4e45\u7684\u90e8\u5206\u662f\u5de5\u4f5c\u5faa\u74b0\uff1a\u5728\u9023\u7e8c\u6eab\u5ea6\u4e0b\u591a\u5c11\u5c0f\u6642\u3001\u6d78\u6ce1\u56de\u6eab\u6703\u8b8a\u5f97\u591a\u71b1\uff0c\u4ee5\u53ca\u8edf\u5316\u5f8c\u7684\u81a0\u6599\u9808\u8de8\u8d8a\u591a\u5c11\u9593\u9699\u3002\u4e00\u500b\u914d\u5099\u6b63\u78ba\u64cb\u5708\u30010.15 mm \u9593\u9699\u53ca\u771f\u5be6\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u9650\u503c\u7684\u6a19\u6e96 FKM \u5bc6\u5c01\u74b0\uff0c\u8868\u73fe\u6703\u52dd\u904e\u4e00\u500b\u786c\u585e\u9032\u70ba\u5ba4\u6eab\u8a2d\u8a08\u7684\u6e9d\u69fd\u4e2d\u7684 FFKM \u5bc6\u5c01\u74b0\u3002<\/p>\n<p>\u628a\u6eab\u5ea6\u4e09\u8981\u7d20\u3001\u6d41\u9ad4\u53ca\u9593\u9699\u767c\u7d66\u6211\u5011\uff0c\u6211\u5011\u4fbf\u6703\u544a\u8a34\u4f60\u9700\u8981\u54ea\u4e00\u7d1a\u968e\u68af\u2014\u2014\u4ee5\u53ca\u54ea\u4e00\u7d1a\u4f60\u53ef\u4ee5\u505c\u6b62\u4ed8\u8cbb\u3002\u700f\u89bd <a href=\"https:\/\/www.bosssealing.com\/zh\/%e7%94%a2%e5%93%81%e5%88%86%e9%a1%9e\/%e9%ab%98%e6%ba%ab%e4%bd%8e%e6%ba%ab%e5%af%86%e5%b0%81%e4%bb%b6\/\">\u9ad8\u4f4e\u6eab\u5bc6\u5c01\u4ef6\u7cfb\u5217<\/a> \u4ee5\u4e86\u89e3\u6a19\u6e96\u578b\u6750\uff0c\u6216\u67e5\u770b <a href=\"https:\/\/www.bosssealing.com\/zh\/%e7%94%a2%e5%93%81%e5%88%86%e9%a1%9e\/%e5%b7%a5%e7%a8%8b%e5%a1%91%e6%96%99%e7%94%a2%e5%93%81\/\">\u6a5f\u52a0\u5de5 PEEK \u53ca PTFE \u96f6\u4ef6<\/a> \uff08\u82e5\u7b54\u6848\u662f\u64cb\u5708\u800c\u975e\u5f48\u6027\u9ad4\uff09\u3002<\/p>\n<p>\u95dc\u65bc\u984d\u5b9a\u503c\u80cc\u5f8c\u7684\u7269\u6599\u79d1\u5b78\uff0cTrelleborg \u767c\u8868\u4e86\u4e00\u4efd\u5be6\u7528\u7684\u6982\u8ff0\uff0c\u4ecb\u7d39 <a href=\"https:\/\/www.trelleborg.com\/en\/seals\/products-and-solutions\" rel=\"noopener\">\u5bc6\u5c01\u6750\u6599\u53ca\u5176\u61c9\u7528\u9650\u5236<\/a>\uff0c\u4ee5\u53ca ASTM <a href=\"https:\/\/www.astm.org\/d2000-12.html\" rel=\"noopener\">D2000<\/a> \u4ecd\u7136\u662f\u5927\u591a\u6578\u7f8e\u570b\u5716\u7d19\u4ecd\u6703\u5f15\u7528\u7684\u7dda\u6a19\u8a3b\u6a19\u6e96\u3002\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u6e2c\u8a66\u7684\u8a73\u7d30\u8cc7\u6599\u8f09\u65bc <a href=\"https:\/\/www.astm.org\/d0395-18.html\" rel=\"noopener\">ASTM D395<\/a>\u3002\u6709\u95dc\u5168\u6c1f\u5f48\u6027\u9ad4\u57fa\u790e\u805a\u5408\u7269\u7684\u6578\u64da\uff0c <a href=\"https:\/\/www.zeon.eu\/\" rel=\"noopener\">Zeon<\/a> \u520a\u8f09\u4e86\u724c\u865f\u7d1a\u5225\u7684\u6eab\u5ea6\u8207\u5316\u5b78\u54c1\u8868\u683c\u3002\u540c\u4e00\u53d6\u6368\u7684\u7d93\u92b7\u5546\u89c0\u9ede\uff08\u4ee5\u7dad\u4fee\u5de5\u7a0b\u5e2b\u800c\u975e\u8a2d\u8a08\u5e2b\u70ba\u5c0d\u8c61\u64b0\u5beb\uff09\u898b\u65bc <a href=\"https:\/\/www.darcoid.com\/materials\" rel=\"nofollow noopener\">Darcoid<\/a>.<\/p>","protected":false},"excerpt":{"rendered":"<p>200 \u00b0C \u5c0d\u5f48\u6027\u9ad4\u6709\u4f55\u5f71\u97ff\u3001\u54ea\u500b\u6750\u6599\u7cfb\u5217\u80fd\u627f\u53d7\uff0c\u4ee5\u53ca\u6bcf\u7a2e\u6750\u6599\u6240\u9700\u7684\u786c\u4ef6\u6539\u52d5\u3002\u9ad8\u6eab\u63a5\u982d\u7684\u9078\u578b\u6d41\u7a0b\u3002<\/p>","protected":false},"author":1,"featured_media":1692,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_monsterinsights_skip_tracking":false,"footnotes":""},"categories":[1],"tags":[],"class_list":["post-1697","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-news"],"aioseo_notices":[],"aioseo_head":"\n\t\t<!-- All in One SEO 5.0.5 - aioseo.com -->\n\t<meta name=\"description\" content=\"Seal materials above 200 C compared: FKM, FFKM, PTFE, PEEK and graphite limits, compression set data, gap and hardware rules, and a selection workflow.\" \/>\n\t<meta name=\"robots\" content=\"max-image-preview:large\" \/>\n\t<meta name=\"author\" content=\"boss\"\/>\n\t<link rel=\"canonical\" href=\"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/\" \/>\n\t\t<meta name=\"generator\" content=\"All in One SEO (AIOSEO) 5.0.5\" \/>\n\t\t<meta property=\"og:locale\" content=\"zh_HK\" \/>\n\t\t<meta property=\"og:site_name\" content=\"BOSS Sealing Solutions - Hydraulic seal and pneumatic seal factory\" \/>\n\t\t<meta property=\"og:type\" content=\"article\" \/>\n\t\t<meta property=\"og:title\" content=\"Seals Above 200 \u00b0C: FKM vs FFKM vs PEEK\" \/>\n\t\t<meta property=\"og:description\" content=\"Seal materials above 200 C compared: FKM, FFKM, PTFE, PEEK and graphite limits, compression set data, gap and hardware rules, and a selection workflow.\" \/>\n\t\t<meta property=\"og:url\" content=\"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/\" \/>\n\t\t<meta property=\"og:image\" content=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png\" \/>\n\t\t<meta property=\"og:image:secure_url\" content=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png\" \/>\n\t\t<meta property=\"article:published_time\" content=\"2026-11-13T07:53:00+00:00\" \/>\n\t\t<meta property=\"article:modified_time\" content=\"2026-11-10T04:00:31+00:00\" \/>\n\t\t<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n\t\t<meta name=\"twitter:title\" content=\"Seals Above 200 \u00b0C: FKM vs FFKM vs PEEK\" \/>\n\t\t<meta name=\"twitter:description\" content=\"Seal materials above 200 C compared: FKM, FFKM, PTFE, PEEK and graphite limits, compression set data, gap and hardware rules, and a selection workflow.\" \/>\n\t\t<meta name=\"twitter:image\" content=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png\" \/>\n\t\t<script type=\"application\/ld+json\" class=\"aioseo-schema\">\n\t\t\t{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"BlogPosting\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#blogposting\",\"name\":\"Seals Above 200 \\u00b0C: FKM vs FFKM vs PEEK\",\"headline\":\"Seals Above 200 \\u00b0C: FKM, FFKM, PEEK and Graphite Options Compared\",\"author\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/#author\"},\"publisher\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#organization\"},\"image\":{\"@type\":\"ImageObject\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/wp-content\\\/uploads\\\/2026\\\/11\\\/a1_hero-2.jpg\",\"width\":1536,\"height\":944,\"caption\":\"High-temperature seal set: brown FKM O-rings, white PTFE rings and PEEK backup rings\"},\"datePublished\":\"2026-11-13T15:53:00+08:00\",\"dateModified\":\"2026-11-10T12:00:31+08:00\",\"inLanguage\":\"zh-HK\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#webpage\"},\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#webpage\"},\"articleSection\":\"Knowledge Base\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#breadcrumblist\",\"itemListElement\":[{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#listItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/\",\"nextItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/category\\\/news\\\/#listItem\",\"name\":\"Knowledge Base\"}},{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/category\\\/news\\\/#listItem\",\"position\":2,\"name\":\"Knowledge Base\",\"item\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/category\\\/news\\\/\",\"nextItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#listItem\",\"name\":\"Seals Above 200 \\u00b0C: FKM, FFKM, PEEK and Graphite Options Compared\"},\"previousItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#listItem\",\"name\":\"Home\"}},{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#listItem\",\"position\":3,\"name\":\"Seals Above 200 \\u00b0C: FKM, FFKM, PEEK and Graphite Options Compared\",\"previousItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/category\\\/news\\\/#listItem\",\"name\":\"Knowledge Base\"}}]},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#organization\",\"name\":\"BOSS Sealing Solutions\",\"description\":\"Hydraulic seal and pneumatic seal factory\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/\",\"email\":\"sales@bosssealing.com\",\"telephone\":\"+86 13392768056\",\"logo\":{\"@type\":\"ImageObject\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/wp-content\\\/uploads\\\/2023\\\/07\\\/logo.png\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#organizationLogo\",\"width\":1744,\"height\":555,\"caption\":\"BOSS Sealing Solutions\"},\"image\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#organizationLogo\"}},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/#author\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/\",\"name\":\"boss\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#webpage\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/\",\"name\":\"Seals Above 200 \\u00b0C: FKM vs FFKM vs PEEK\",\"description\":\"Seal materials above 200 C compared: FKM, FFKM, PTFE, PEEK and graphite limits, compression set data, gap and hardware rules, and a selection workflow.\",\"inLanguage\":\"zh-HK\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#website\"},\"breadcrumb\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#breadcrumblist\"},\"author\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/#author\"},\"creator\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/#author\"},\"image\":{\"@type\":\"ImageObject\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/wp-content\\\/uploads\\\/2026\\\/11\\\/a1_hero-2.jpg\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#mainImage\",\"width\":1536,\"height\":944,\"caption\":\"High-temperature seal set: brown FKM O-rings, white PTFE rings and PEEK backup rings\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/seals-above-200c\\\/#mainImage\"},\"datePublished\":\"2026-11-13T15:53:00+08:00\",\"dateModified\":\"2026-11-10T12:00:31+08:00\"},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#website\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/\",\"name\":\"BOSS Sealing Solutions\",\"alternateName\":\"BOSS Sealing\",\"description\":\"Hydraulic seal and pneumatic seal factory\",\"inLanguage\":\"zh-HK\",\"publisher\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#organization\"}}]}\n\t\t<\/script>\n\t\t<!-- All in One SEO -->\n\n","aioseo_head_json":{"title":"200 \u00b0C \u4ee5\u4e0a\u7684\u5bc6\u5c01\u4ef6\uff1aFKM \u8207 FFKM \u8207 PEEK \u7684\u6bd4\u8f03","description":"\u6bd4\u8f03 200\u00b0C \u4ee5\u4e0a\u7684\u5bc6\u5c01\u6750\u6599\uff1aFKM\u3001FFKM\u3001PTFE\u3001PEEK \u8207\u77f3\u58a8\u7684\u6975\u9650\u3001\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u6578\u64da\u3001\u9593\u9699\u8207\u786c\u4ef6\u898f\u5247\uff0c\u4ee5\u53ca\u9078\u578b\u6d41\u7a0b\u3002","canonical_url":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/","robots":"max-image-preview:large","keywords":"","webmasterTools":{"miscellaneous":""},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"BlogPosting","@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#blogposting","name":"Seals Above 200 \u00b0C: FKM vs FFKM vs PEEK","headline":"Seals Above 200 \u00b0C: FKM, FFKM, PEEK and Graphite Options Compared","author":{"@id":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/#author"},"publisher":{"@id":"https:\/\/www.bosssealing.com\/zh\/#organization"},"image":{"@type":"ImageObject","url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2026\/11\/a1_hero-2.jpg","width":1536,"height":944,"caption":"High-temperature seal set: brown FKM O-rings, white PTFE rings and PEEK backup rings"},"datePublished":"2026-11-13T15:53:00+08:00","dateModified":"2026-11-10T12:00:31+08:00","inLanguage":"zh-HK","mainEntityOfPage":{"@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#webpage"},"isPartOf":{"@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#webpage"},"articleSection":"Knowledge Base"},{"@type":"BreadcrumbList","@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#breadcrumblist","itemListElement":[{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/#listItem","position":1,"name":"Home","item":"https:\/\/www.bosssealing.com\/zh\/","nextItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/category\/news\/#listItem","name":"Knowledge Base"}},{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/category\/news\/#listItem","position":2,"name":"Knowledge Base","item":"https:\/\/www.bosssealing.com\/zh\/category\/news\/","nextItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#listItem","name":"Seals Above 200 \u00b0C: FKM, FFKM, PEEK and Graphite Options Compared"},"previousItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/#listItem","name":"Home"}},{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#listItem","position":3,"name":"Seals Above 200 \u00b0C: FKM, FFKM, PEEK and Graphite Options Compared","previousItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/category\/news\/#listItem","name":"Knowledge Base"}}]},{"@type":"Organization","@id":"https:\/\/www.bosssealing.com\/zh\/#organization","name":"BOSS Sealing Solutions","description":"Hydraulic seal and pneumatic seal factory","url":"https:\/\/www.bosssealing.com\/zh\/","email":"sales@bosssealing.com","telephone":"+86 13392768056","logo":{"@type":"ImageObject","url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#organizationLogo","width":1744,"height":555,"caption":"BOSS Sealing Solutions"},"image":{"@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#organizationLogo"}},{"@type":"Person","@id":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/#author","url":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/","name":"boss"},{"@type":"WebPage","@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#webpage","url":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/","name":"Seals Above 200 \u00b0C: FKM vs FFKM vs PEEK","description":"Seal materials above 200 C compared: FKM, FFKM, PTFE, PEEK and graphite limits, compression set data, gap and hardware rules, and a selection workflow.","inLanguage":"zh-HK","isPartOf":{"@id":"https:\/\/www.bosssealing.com\/zh\/#website"},"breadcrumb":{"@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#breadcrumblist"},"author":{"@id":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/#author"},"creator":{"@id":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/#author"},"image":{"@type":"ImageObject","url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2026\/11\/a1_hero-2.jpg","@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#mainImage","width":1536,"height":944,"caption":"High-temperature seal set: brown FKM O-rings, white PTFE rings and PEEK backup rings"},"primaryImageOfPage":{"@id":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/#mainImage"},"datePublished":"2026-11-13T15:53:00+08:00","dateModified":"2026-11-10T12:00:31+08:00"},{"@type":"WebSite","@id":"https:\/\/www.bosssealing.com\/zh\/#website","url":"https:\/\/www.bosssealing.com\/zh\/","name":"BOSS Sealing Solutions","alternateName":"BOSS Sealing","description":"Hydraulic seal and pneumatic seal factory","inLanguage":"zh-HK","publisher":{"@id":"https:\/\/www.bosssealing.com\/zh\/#organization"}}]},"og:locale":"zh_HK","og:site_name":"BOSS Sealing Solutions - Hydraulic seal and pneumatic seal factory","og:type":"article","og:title":"Seals Above 200 \u00b0C: FKM vs FFKM vs PEEK","og:description":"Seal materials above 200 C compared: FKM, FFKM, PTFE, PEEK and graphite limits, compression set data, gap and hardware rules, and a selection workflow.","og:url":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/","og:image":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","og:image:secure_url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","article:published_time":"2026-11-13T07:53:00+00:00","article:modified_time":"2026-11-10T04:00:31+00:00","twitter:card":"summary_large_image","twitter:title":"Seals Above 200 \u00b0C: FKM vs FFKM vs PEEK","twitter:description":"Seal materials above 200 C compared: FKM, FFKM, PTFE, PEEK and graphite limits, compression set data, gap and hardware rules, and a selection workflow.","twitter:image":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png"},"aioseo_meta_data":{"post_id":"1697","title":"200 \u00b0C \u4ee5\u4e0a\u7684\u5bc6\u5c01\u4ef6\uff1aFKM \u8207 FFKM \u8207 PEEK \u7684\u6bd4\u8f03","description":"\u6bd4\u8f03 200\u00b0C \u4ee5\u4e0a\u7684\u5bc6\u5c01\u6750\u6599\uff1aFKM\u3001FFKM\u3001PTFE\u3001PEEK \u8207\u77f3\u58a8\u7684\u6975\u9650\u3001\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\u6578\u64da\u3001\u9593\u9699\u8207\u786c\u4ef6\u898f\u5247\uff0c\u4ee5\u53ca\u9078\u578b\u6d41\u7a0b\u3002","keywords":null,"keyphrases":{"focus":{"keyphrase":"","score":0,"analysis":{"keyphraseInTitle":{"score":0,"maxScore":9,"error":1}}},"additional":[]},"primary_term":null,"canonical_url":null,"og_title":null,"og_description":null,"og_object_type":"default","og_image_type":"default","og_image_url":null,"og_image_width":null,"og_image_height":null,"og_image_custom_url":null,"og_image_custom_fields":null,"og_video":"","og_custom_url":null,"og_article_section":null,"og_article_tags":null,"twitter_use_og":false,"twitter_card":"default","twitter_image_type":"default","twitter_image_url":null,"twitter_image_custom_url":null,"twitter_image_custom_fields":null,"twitter_title":null,"twitter_description":null,"schema":{"blockGraphs":[],"customGraphs":[],"default":{"data":{"Article":[],"Course":[],"Dataset":[],"FAQPage":[],"Movie":[],"Person":[],"Product":[],"ProductReview":[],"Car":[],"Recipe":[],"Service":[],"SoftwareApplication":[],"WebPage":[]},"graphName":"BlogPosting","isEnabled":true},"graphs":[]},"schema_type":"default","schema_type_options":null,"pillar_content":false,"robots_default":true,"robots_noindex":false,"robots_noarchive":false,"robots_nosnippet":false,"robots_nofollow":false,"robots_noimageindex":false,"robots_noodp":false,"robots_notranslate":false,"robots_max_snippet":"-1","robots_max_videopreview":"-1","robots_max_imagepreview":"large","priority":null,"frequency":"default","local_seo":null,"breadcrumb_settings":null,"limit_modified_date":false,"ai":{"faqs":[],"keyPoints":[],"schemas":[],"titles":[],"descriptions":[],"socialPosts":{"email":[],"linkedin":[],"twitter":[],"facebook":[],"instagram":[]}},"created":"2026-11-10 04:49:49","updated":"2026-11-13 08:27:56","seo_analyzer_scan_date":null,"focus_keyword":null,"additional_keywords":null,"truseo_locale":null},"aioseo_breadcrumb":"<div class=\"aioseo-breadcrumbs\"><span class=\"aioseo-breadcrumb\">\n\t\t\t<a href=\"https:\/\/www.bosssealing.com\/zh\/\" title=\"Home\">Home<\/a>\n\t\t<\/span><span class=\"aioseo-breadcrumb-separator\">\u00bb<\/span><span class=\"aioseo-breadcrumb\">\n\t\t\t<a href=\"https:\/\/www.bosssealing.com\/zh\/category\/news\/\" title=\"Knowledge Base\">Knowledge Base<\/a>\n\t\t<\/span><span class=\"aioseo-breadcrumb-separator\">\u00bb<\/span><span class=\"aioseo-breadcrumb\">\n\t\t\tSeals Above 200 \u00b0C: FKM, FFKM, PEEK and Graphite Options Compared\n\t\t<\/span><\/div>","aioseo_breadcrumb_json":[{"label":"Home","link":"https:\/\/www.bosssealing.com\/zh\/"},{"label":"Knowledge Base","link":"https:\/\/www.bosssealing.com\/zh\/category\/news\/"},{"label":"Seals Above 200 \u00b0C: FKM, FFKM, PEEK and Graphite Options Compared","link":"https:\/\/www.bosssealing.com\/zh\/seals-above-200c\/"}],"_links":{"self":[{"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/posts\/1697","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/comments?post=1697"}],"version-history":[{"count":1,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/posts\/1697\/revisions"}],"predecessor-version":[{"id":1742,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/posts\/1697\/revisions\/1742"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/media\/1692"}],"wp:attachment":[{"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/media?parent=1697"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/categories?post=1697"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/tags?post=1697"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}