{"id":1649,"date":"2026-11-03T20:43:00","date_gmt":"2026-11-03T12:43:00","guid":{"rendered":"https:\/\/www.bosssealing.com\/?p=1649"},"modified":"2026-11-03T20:43:00","modified_gmt":"2026-11-03T12:43:00","slug":"%e6%b6%b2%e5%a3%93%e5%af%86%e5%b0%81%e4%bb%b6%e5%a4%b1%e6%95%88%e5%8e%9f%e5%9b%a0","status":"publish","type":"post","link":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/","title":{"rendered":"\u6db2\u58d3\u5bc6\u5c01\u4ef6\u5931\u6548\u7684\u5341\u5927\u539f\u56e0\u53ca\u9010\u4e00\u9810\u9632\u65b9\u6cd5"},"content":{"rendered":"<p>\u6bcf\u4e00\u6b21\u6db2\u58d3\u5bc6\u5c01\u5931\u6548\u90fd\u6703\u7559\u4e0b\u8b49\u64da\u3002\u640d\u58de\u7684\u5f62\u72c0\u3001\u5728\u5507\u908a\u4e0a\u7684\u4f4d\u7f6e\uff0c\u4ee5\u53ca\u914d\u5408\u91d1\u5c6c\u7684\u72c0\u6cc1\uff0c\u90fd\u80fd\u5728\u6cb9\u6db2\u5206\u6790\u7d50\u679c\u51fa\u4f86\u4e4b\u524d\u5f88\u4e45\u5c31\u544a\u8a34\u4f60\u767c\u751f\u4e86\u4ec0\u9ebc\u4e8b\u3002\u554f\u984c\u5728\u65bc\uff0c\u5927\u591a\u6578\u7dad\u4fee\u5718\u968a\u53ea\u662f\u66f4\u63db\u5bc6\u5c01\u4ef6\u3001\u88dc\u5145\u6cb9\u6db2\u7136\u5f8c\u7e7c\u7e8c\u904b\u4f5c\uff0c\u7d50\u679c\u540c\u6a23\u7684\u6545\u969c\u5e7e\u9031\u5167\u53c8\u518d\u51fa\u73fe\u3002<\/p>\n<p>\u6211\u5011\u70ba\u5efa\u7bc9\u3001\u8fb2\u696d\u53ca\u5de5\u696d\u8a2d\u5099\u9818\u57df\u7684\u5ba2\u6236\u7ffb\u65b0\u53ca\u91cd\u65b0\u5bc6\u5c01\u6cb9\u7f38\uff0c\u800c\u6211\u5011\u6240\u898b\u7684\u5e7e\u4e4e\u6bcf\u4e00\u6b21\u63d0\u65e9\u5931\u6548\uff0c\u90fd\u53ef\u6b78\u56e0\u65bc\u540c\u6a23\u7684\u5341\u500b\u539f\u56e0\u3002\u4ee5\u4e0b\u9010\u4e00\u8aaa\u660e\u6bcf\u500b\u539f\u56e0\u53ca\u5176\u7559\u4e0b\u7684\u7269\u7406\u7279\u5fb5\uff0c\u4e26\u6309\u7cfb\u7d71\u4e2d\u7522\u751f\u8a72\u554f\u984c\u7684\u90e8\u5206\u5206\u7d44\uff1a\u6c61\u67d3\u7269\u3001\u71b1\u8207\u5316\u5b78\uff0c\u4ee5\u53ca\u6a5f\u68b0\u8ca0\u8377\u3002<\/p>\n<h2>\u5f9e\u640d\u58de\u60c5\u6cc1\u5165\u624b\uff0c\u800c\u975e\u96f6\u4ef6\u7de8\u865f<\/h2>\n<p>\u5728\u8a02\u8cfc\u66ff\u63db\u4ef6\u4e4b\u524d\uff0c\u5148\u8b80\u61c2\u4f60\u62c6\u4e0b\u4f86\u7684\u5bc6\u5c01\u4ef6\u3002\u4e0b\u8868\u5c07\u6700\u5e38\u898b\u7684\u5916\u89c0\u5c0d\u61c9\u5230\u5176\u6210\u56e0\u3002\u6e05\u6f54\u524d\u5148\u70ba\u5bc6\u5c01\u4ef6\u62cd\u7167\uff1b\u64e6\u62ed\u5507\u908a\u6703\u7834\u58de\u8b49\u64da\u3002<\/p>\n<table>\n<thead>\n<tr>\n<th>\u5bc6\u5c01\u4ef6\u4e0a\u770b\u5230\u7684\u60c5\u6cc1<\/th>\n<th>\u6700\u53ef\u80fd\u7684\u539f\u56e0<\/th>\n<th>\u9996\u5148\u61c9\u6aa2\u67e5\u7684\u4e8b\u9805<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>\u4f4e\u58d3\u5074\u6709\u4e00\u908a\u88ab\u5543\u54ac\u6216\u7f3a\u640d<\/td>\n<td>\u9593\u9699\u904e\u5927\u5c0e\u81f4\u64e0\u51fa<\/td>\n<td>\u586b\u6599\u51fd\u9593\u9699\u53ca\u662f\u5426\u6709\u64cb\u5708<\/td>\n<\/tr>\n<tr>\n<td>\u5507\u908a\u786c\u5316\u3001\u9f9c\u88c2\u3001\u767c\u4eae\u6216\u8d77\u6ce1<\/td>\n<td>\u6eab\u5ea6\u904e\u9ad8<\/td>\n<td>\u6cb9\u7f38\u8655\u7684\u6cb9\u6db2\u6eab\u5ea6\u3001\u51b7\u537b\u5668\u6548\u80fd<\/td>\n<\/tr>\n<tr>\n<td>\u5bc6\u5c01\u4ef6\u81a8\u8139\u3001\u8b8a\u8edf\u3001\u767c\u9ecf\u6216\u8d77\u6ce1<\/td>\n<td>\u81a0\u6599\u8207\u6cb9\u6db2\u4e0d\u76f8\u5bb9<\/td>\n<td>\u6cb9\u6db2\u985e\u578b\u53ca\u6dfb\u52a0\u5291\u914d\u65b9\u5c0d\u6bd4\u6750\u6599\u6578\u64da<\/td>\n<\/tr>\n<tr>\n<td>\u5507\u908a\u5468\u570d\u5747\u52fb\u78e8\u640d\uff0c\u7121\u522e\u75d5<\/td>\n<td>\u6b63\u5e38\u4f7f\u7528\u58fd\u547d<\/td>\n<td>\u7d2f\u8a08\u904b\u884c\u6642\u6578\u53ca\u6cb9\u6db2\u6e05\u6f54\u5ea6\u8a18\u9304<\/td>\n<\/tr>\n<tr>\n<td>\u78e8\u640d\u96c6\u4e2d\u5728\u5713\u5468\u7684\u4e00\u5074<\/td>\n<td>\u5074\u5411\u8ca0\u8377\u6216\u5c0d\u4f4d\u4e0d\u826f<\/td>\n<td>\u6d3b\u585e\u687f\u504f\u64fa\u3001\u896f\u5957\u78e8\u640d\u3001\u6cb9\u7f38\u5b89\u88dd<\/td>\n<\/tr>\n<tr>\n<td>\u5713\u5468\u65b9\u5411\u6709\u6df1\u522e\u75d5\uff0c\u5d4c\u5165\u91d1\u5c6c<\/td>\n<td>\u78e8\u8755\u6027\u6c61\u67d3\u7269<\/td>\n<td>\u9632\u5875\u5708\u72c0\u6cc1\u3001\u547c\u5438\u5668\u3001\u904e\u6ffe\u3001\u6cb9\u6db2 ISO \u7b49\u7d1a<\/td>\n<\/tr>\n<tr>\n<td>\u58d3\u6241\u3001\u5b9a\u578b\uff0c\u64e0\u58d3\u6642\u7121\u56de\u5f48\u529b<\/td>\n<td>\u56e0\u9ad8\u6eab\u6216\u58d3\u7e2e\u91cf\u904e\u5927\u9020\u6210\u7684\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62<\/td>\n<td>\u6e9d\u69fd\u6df1\u5ea6\u53ca\u5de5\u4f5c\u6eab\u5ea6<\/td>\n<\/tr>\n<tr>\n<td>\u5507\u908a\u6709\u87ba\u65cb\u72c0\u6216\u659c\u5411\u5207\u53e3<\/td>\n<td>\u5b89\u88dd\u640d\u58de<\/td>\n<td>\u7d44\u88dd\u6280\u8853\u3001\u6e9d\u69fd\u908a\u7de3\u5713\u89d2\u3001\u5de5\u5177<\/td>\n<\/tr>\n<tr>\n<td>\u5bc6\u5c01\u4ef6\u88ab\u64e0\u51fa\u6e9d\u69fd<\/td>\n<td>\u5bc6\u5c01\u4ef6\u5f8c\u65b9\u56f0\u4f4f\u58d3\u529b\uff0c\u6216\u7f3a\u5c11\u56fa\u5b9a\u74b0<\/td>\n<td>\u6392\u6db2\u901a\u9053\u53ca\u6e9d\u69fd\u56fa\u5b9a<\/td>\n<\/tr>\n<tr>\n<td>\u586b\u6599\u51fd\u5167\u6709\u9ed1\u8272\u6cb9\u6ce5\u53ca\u6a61\u81a0\u788e\u5c51<\/td>\n<td>\u56b4\u91cd\u52a3\u5316\uff0c\u901a\u5e38\u70ba\u6c61\u67d3\u7269\u52a0\u4e0a\u9ad8\u6eab<\/td>\n<td>\u6cb9\u6db2\u72c0\u6cc1\u53ca\u6574\u500b\u7cfb\u7d71\u6c96\u6d17<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<figure class=\"wp-block-image size-large\"><img decoding=\"async\" src=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2026\/11\/rod_seal_failure.jpg\" alt=\"\u5931\u6548\u7684\u805a\u6c28\u916f\u6db2\u58d3\u6d3b\u585e\u687f\u5bc6\u5c01\u4ef6\uff0c\u5507\u53e3\u6495\u88c2\uff0c\u65c1\u908a\u653e\u6709\u5361\u5c3a\u53ca\u78e8\u640d\u7684\u934d\u927b\u6d3b\u585e\u687f\" \/><figcaption>\u4e00\u500b\u63d0\u65e9\u5931\u6548\u5f8c\u62c6\u4e0b\u7684\u6d3b\u585e\u687f\u5bc6\u5c01\u4ef6\uff1a\u7834\u640d\u3001\u88ab\u5543\u54ac\u7684\u5507\u908a\u53ca\u788e\u5c51\u5c31\u662f\u8b49\u64da\uff0c\u800c\u5f9e\u640d\u58de\u6a21\u5f0f\u5373\u53ef\u8b80\u51fa\u6210\u56e0<\/figcaption><\/figure>\n<h2>\u7b2c\u4e00\u7d44\uff1a\u6c61\u67d3\u7269<\/h2>\n<h3>1. \u6cb9\u6db2\u4e2d\u7684\u78e8\u8755\u6027\u9846\u7c92<\/h3>\n<p>\u5728\u6211\u5011\u6240\u898b\u7684\u6bcf\u4e00\u9805\u8eca\u968a\u7814\u7a76\u4e2d\uff0c\u9019\u90fd\u662f\u5bc6\u5c01\u4ef6\u63d0\u65e9\u5931\u6548\u7684\u9996\u8981\u539f\u56e0\uff0c\u800c\u4e14\u5e7e\u4e4e\u7e3d\u662f\u4eba\u70ba\u9020\u6210\u30024 \u81f3 20 \u00b5m \u7684\u9846\u7c92\u6703\u7a7f\u904e\u586b\u6599\u51fd\u9593\u9699\uff0c\u5728\u5bc6\u5c01\u5507\u908a\u4e0a\u8d77\u7814\u78e8\u5291\u7684\u4f5c\u7528\u3002\u5bc6\u5c01\u4ef6\u7531\u5916\u5411\u5167\u78e8\u640d\uff0c\u9593\u9699\u96a8\u4e4b\u589e\u5927\uff0c\u66f4\u591a\u9846\u7c92\u9032\u5165\uff0c\u5931\u6548\u4fbf\u52a0\u901f\u3002<\/p>\n<p>\u5176\u7279\u5fb5\u662f\u5507\u908a\u5747\u52fb\u78e8\u8584\uff0c\u5448\u62cb\u5149\u3001\u767c\u4eae\u7684\u5916\u89c0\uff0c\u6d3b\u585e\u687f\u4e0a\u6709\u7d30\u5fae\u7684\u5713\u5468\u522e\u75d5\u3002\u6cb9\u6db2\u5206\u6790\u901a\u5e38\u986f\u793a ISO 4406 \u7b49\u7d1a\u9ad8\u65bc 19\/17\/14\uff0c\u800c\u76ee\u6a19\u70ba 18\/16\/13 \u6216\u66f4\u597d\u3002\u89e3\u6c7a\u4e4b\u9053\u5728\u65bc\u904e\u6ffe\u8207\u73fe\u5834\u7ba1\u7406\uff0c\u800c\u975e\u6539\u7528\u4e0d\u540c\u7684\u5bc6\u5c01\u81a0\u6599\u3002<\/p>\n<h3>2. \u9632\u5875\u5708\u5931\u6548\u6216\u7f3a\u5931<\/h3>\n<p>\u9632\u5875\u5708\u662f\u552f\u4e00\u80fd\u963b\u6b62\u5916\u90e8\u6c61\u57a2\u9032\u5165\u6cb9\u7f38\u7684\u96f6\u4ef6\u3002\u5507\u908a\u7834\u640d\u3001\u9632\u5875\u5708\u5f9e\u6e9d\u69fd\u4e2d\u7ff9\u8d77\uff0c\u6216\u5728\u4e0a\u6b21\u7ffb\u65b0\u6642\u88ab\u7701\u7565\uff0c\u90fd\u6703\u4f7f\u6d3b\u585e\u687f\u8b8a\u6210\u8f38\u9001\u7070\u5875\u8207\u7802\u792b\u7684\u8f38\u9001\u5e36\u3002\u6d3b\u585e\u687f\u5bc6\u5c01\u4ef6\u63a5\u8457\u6703\u5728\u9060\u4f4e\u65bc\u9810\u671f\u58fd\u547d\u7684\u6642\u9593\u5167\u5931\u6548\uff0c\u800c\u9019\u985e\u5931\u6548\u5f80\u5f80\u88ab\u6b78\u548e\u65bc\u6d3b\u585e\u687f\u5bc6\u5c01\u4ef6\u3002<\/p>\n<p>\u5728\u6bcf\u500b\u4fdd\u990a\u9031\u671f\u6aa2\u67e5\u9632\u5875\u5708\uff0c\u800c\u975e\u6bcf\u6b21\u7ffb\u65b0\u624d\u6aa2\u67e5\u3002\u5728\u7c89\u5875\u74b0\u5883\u4e2d\u4f5c\u696d\u7684\u79fb\u52d5\u8a2d\u5099\u4e0a\uff0c\u908a\u7de3\u7ff9\u8d77\u7684\u9632\u5875\u5708\u61c9\u5728\u4e0b\u4e00\u6b21\u53ef\u505c\u6a5f\u6642\u66f4\u63db\uff0c\u800c\u975e\u7b49\u5230\u4e0b\u4e00\u6b21\u6392\u5b9a\u7684\u7ffb\u4fee\u3002\u6211\u5011\u7684 <a href=\"https:\/\/www.bosssealing.com\/zh\/%e7%94%a2%e5%93%81%e5%88%86%e9%a1%9e\/%e6%b6%b2%e5%a3%93%e5%88%ae%e5%a1%b5%e5%af%86%e5%b0%81%e4%bb%b6\/\">\u9632\u5875\u5708\u7cfb\u5217<\/a> \u6db5\u84cb\u55ae\u5507\u53ca\u96d9\u5507\u578b\u865f\uff0c\u5305\u62ec\u914d\u5099\u91d1\u5c6c\u5916\u6bbc\u3001\u9069\u7528\u65bc\u9ad8\u78e8\u8755\u5de5\u6cc1\u7684\u7248\u672c\u3002<\/p>\n<h3>3. \u53d7\u6c61\u67d3\u7684\u65b0\u6cb9\u53ca\u4e0d\u6f54\u7684\u7d44\u88dd<\/h3>\n<p>\u5f9e\u6cb9\u6876\u53d6\u51fa\u7684\u65b0\u6cb9\u4e26\u975e\u6f54\u6de8\u7684\u6cb9\u3002\u5b83\u7d93\u5e38\u6e2c\u51fa\u6bd4\u7cfb\u7d71\u76ee\u6a19\u9ad2\u5169\u500b ISO \u7b49\u7d1a\uff0c\u56e0\u6b64\u6bcf\u6b21\u900f\u904e\u958b\u653e\u5f0f\u6f0f\u6597\u88dc\u5145\u6cb9\u6db2\uff0c\u90fd\u6703\u62b5\u92b7\u6578\u500b\u6708\u7684\u904e\u6ffe\u6210\u679c\u3002\u7d44\u88dd\u9084\u6703\u5e36\u4f86\u7b2c\u4e8c\u91cd\u6c61\u67d3\uff1a\u5728\u4f48\u6eff\u7814\u78e8\u7c89\u5875\u7684\u5de5\u4f5c\u53f0\u4e0a\u5b89\u88dd\u5bc6\u5c01\u4ef6\uff0c\u6216\u7528\u8eca\u9593\u62b9\u5e03\u64e6\u62ed\u586b\u6599\u51fd\uff0c\u90fd\u6703\u5c07\u9846\u7c92\u76f4\u63a5\u5e36\u5165\u5bc6\u5c01\u5340\u57df\u3002<\/p>\n<p>\u89e3\u6c7a\u65b9\u6cd5\u5728\u65bc\u7a0b\u5e8f\u3002\u904e\u6ffe\u9032\u5165\u6a5f\u5668\u7684\u6bcf\u4e00\u516c\u5347\u6db2\u9ad4\uff0c\u8edf\u7ba1\u4e00\u62c6\u4e0b\u5c31\u7acb\u5373\u5c01\u53e3\uff0c\u4e26\u5728\u4e7e\u6de8\u7684\u588a\u4e0a\u7d44\u88dd\uff0c\u5bc6\u5c01\u4ef6\u5728\u88dd\u914d\u524d\u4e00\u523b\u4ecd\u7559\u5728\u5176\u5305\u88dd\u5167\u3002<\/p>\n<h2>\u7b2c 2 \u7d44\uff1a\u71b1\u8207\u5316\u5b78<\/h2>\n<h3>4. \u5728\u8d85\u904e\u5316\u5408\u7269\u6eab\u5ea6\u4e0a\u9650\u4e0b\u904b\u4f5c<\/h3>\n<p>\u6bcf\u7a2e\u5f48\u6027\u9ad4\u90fd\u6709\u4e00\u500b\u4e0a\u9650\uff0c\u8d85\u904e\u6b64\u4e0a\u9650\u4fbf\u6703\u786c\u5316\u3001\u5931\u53bb\u5f48\u6027\u4e26\u7522\u751f\u6c38\u4e45\u8b8a\u5f62\u3002NBR \u7d04\u53ef\u627f\u53d7\u81f3 100 \u00b0C\uff0cPU \u7d04\u81f3 90 \u00b0C\uff0cFKM \u7d04\u81f3 200 \u00b0C\u3002\u4ee5 NBR \u5bc6\u5c01\u4ef6\u5728 110 \u00b0C \u4e0b\u904b\u4f5c\u7684\u6cb9\u7f38\uff0c\u6703\u5728\u6578\u767e\u5c0f\u6642\u5167\u51fa\u73fe\u786c\u5316\u3001\u9f9c\u88c2\u7684\u5507\u908a\u53ca\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\uff0c\u4efb\u4f55\u5b89\u88dd\u6280\u8853\u90fd\u7121\u6cd5\u907f\u514d\u3002\u82e5\u5fc5\u9808\u63d0\u9ad8\u4e0a\u9650\uff0cHNBR \u901a\u5e38\u662f\u7b2c\u4e00\u6b65\u5347\u7d1a\uff1a <a href=\"https:\/\/www.zeon.eu\/\">Zeon<\/a>\uff0c\u8a72\u516c\u53f8\u5c07 HNBR \u5546\u54c1\u5316\u70ba Zetpol\uff0c\u4e26\u516c\u5e03\u5927\u591a\u6578\u5bc6\u5c01\u4ef6\u6210\u578b\u5546\u6240\u4f9d\u64da\u7684\u81a0\u6599\u7b49\u7d1a\u3002<\/p>\n<table>\n<thead>\n<tr>\n<th>\u6750\u6599<\/th>\n<th>\u9023\u7e8c\u7bc4\u570d<\/th>\n<th>\u77ed\u671f\u5cf0\u503c<\/th>\n<th>\u8d85\u51fa\u6642\u5605\u5931\u6548\u7279\u5fb5<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>\u4e01\u8148\u6a61\u81a0<\/td>\n<td>\u221230 \u81f3 +100 \u00b0C<\/td>\n<td>120 \u00b0C<\/td>\n<td>\u786c\u5316\u3001\u9f9c\u88c2\u7684\u5507\u908a\uff1b\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62\uff1b\u984f\u8272\u8b8a\u6df1<\/td>\n<\/tr>\n<tr>\n<td>HNBR<\/td>\n<td>\u221230 \u81f3 +150 \u00b0C<\/td>\n<td>160 \u00b0C<\/td>\n<td>\u786c\u5316\uff0c\u4f46\u9f9c\u88c2\u60c5\u6cc1\u8f03 NBR \u5c11<\/td>\n<\/tr>\n<tr>\n<td>\u6c1f\u6a61\u81a0<\/td>\n<td>\u221220 \u81f3 +200 \u00b0C<\/td>\n<td>230 \u00b0C<\/td>\n<td>\u5507\u908a\u8b8a\u8106\u3001\u5e36\u85cd\u8272\u5149\u6fa4\u3001\u6df1\u5c64\u9f9c\u88c2<\/td>\n<\/tr>\n<tr>\n<td>\u805a\u6c28\u916f<\/td>\n<td>\u221230 \u81f3 +90 \u00b0C<\/td>\n<td>100 \u00b0C<\/td>\n<td>\u8edf\u5316\uff0c\u7136\u5f8c\u9084\u539f\u6210\u9ecf\u7a20\u7269\u8cea<\/td>\n<\/tr>\n<tr>\n<td>\u805a\u56db\u6c1f\u4e59\u70ef<\/td>\n<td>\u2212200 \u81f3 +260 \u00b0C<\/td>\n<td>300 \u00b0C<\/td>\n<td>\u8b8a\u5f62\u53ca\u51b7\u6d41\uff0c\u800c\u975e\u9f9c\u88c2<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u5728\u5bc6\u5c01\u4ef6\u8655\u91cf\u5ea6\u6eab\u5ea6\uff0c\u800c\u975e\u5728\u6cb9\u7bb1\u8655\u3002\u9760\u8fd1\u7194\u7210\u3001\u58d3\u9444\u6a5f\u6216\u5f15\u64ce\u6b67\u7ba1\u7684\u6cb9\u7f38\uff0c\u6eab\u5ea6\u53ef\u6bd4\u6cb9\u7bb1\u9ad8 40 \u00b0C\u3002\u82e5\u6d41\u9ad4\u672c\u8eab\u9ad8\u6eab\uff0c\u52a0\u88dd\u98a8\u51b7\u5668\u6216\u52a0\u5927\u6cb9\u7bb1\u6bd4\u63a1\u7528\u9ad8\u7d1a\u81a0\u6599\u66f4\u80fd\u89e3\u6c7a\u554f\u984c\u3002\u82e5\u554f\u984c\u5728\u65bc\u74b0\u5883\u71b1\uff0c\u9694\u71b1\u7f69\u6bd4 FKM \u66f4\u4fbf\u5b9c\u3002\u5c0d\u65bc\u975e\u7d14\u7926\u7269\u6cb9\u7684\u6d41\u9ad4\uff0c\u4f86\u81ea\u4ee5\u4e0b\u7d93\u92b7\u5546\u7684\u76f8\u5bb9\u6027\u5716\u8868\uff0c\u4f8b\u5982 <a href=\"https:\/\/www.darcoid.com\/\" rel=\"nofollow noopener\">Darcoid<\/a> \uff0c\u53ef\u4f5c\u70ba\u5c0d\u4f9b\u61c9\u5546\u81ea\u8eab\u8072\u660e\u7684\u6709\u7528\u4ea4\u53c9\u6838\u5c0d\u3002<\/p>\n<h3>5. \u81a0\u6599\u8207\u6d41\u9ad4\u4e0d\u5339\u914d<\/h3>\n<p>\u5316\u5b78\u4e0d\u76f8\u5bb9\u5c0e\u81f4\u7684\u5bc6\u5c01\u5931\u6548\u8207\u71b1\u5931\u6548\u770b\u8d77\u4f86\u4e0d\u540c\uff1a\u5bc6\u5c01\u4ef6\u6703\u81a8\u8139\u3001\u8edf\u5316\u3001\u8d77\u6ce1\u6216\u90e8\u5206\u6eb6\u89e3\u3002NBR \u5728\u78f7\u9178\u916f\u6d41\u9ad4\u4e2d\u6703\u56b4\u91cd\u81a8\u8139\u3002EPDM \u5728\u7926\u7269\u6cb9\u4e2d\u6703\u89e3\u9ad4\u3002PU \u5728\u6c34\u6027\u6d41\u9ad4\u4e2d\u6703\u6c34\u89e3\u4e26\u8b8a\u6210\u7c89\u72c0\u3002FKM \u5728\u5927\u591a\u6578\u7926\u7269\u6cb9\u4e2d\u8868\u73fe\u512a\u7570\uff0c\u4f46\u5728\u916e\u985e\u3001\u916f\u985e\u53ca\u4f4e\u5206\u5b50\u91cf\u80fa\u985e\u4e2d\u8868\u73fe\u6b20\u4f73\u3002<\/p>\n<p>\u9019\u7a2e\u5931\u6548\u6613\u65bc\u9810\u9632\uff0c\u4e5f\u6613\u65bc\u8aa4\u8a3a\uff0c\u56e0\u70ba\u81a8\u8139\u7684\u5bc6\u5c01\u4ef6\u5728\u62c6\u4e0b\u6642\u4ecd\u53ef\u80fd\u770b\u4f3c\u5b8c\u597d\u3002\u5c07\u62c6\u4e0b\u7684\u5bc6\u5c01\u4ef6\u5c3a\u5bf8\u8207\u65b0\u7684\u6bd4\u8f03\uff1a\u622a\u9762\u589e\u9577\u8d85\u904e\u7d04 5% \u5373\u8868\u793a\u5438\u6536\uff0c\u7121\u8ad6\u6578\u64da\u8868\u5982\u4f55\u8072\u7a31\uff0c\u81a0\u6599\u90fd\u662f\u932f\u7684\u3002\u6309 <a href=\"https:\/\/www.astm.org\/standards\/d2000\">ASTM D2000<\/a> \u64b0\u5beb\u7684\u81a0\u6599\u6a19\u8a3b\u4f7f\u9019\u7a2e\u6bd4\u8f03\u6210\u70ba\u53ef\u80fd\uff1b\u800c\u7c60\u7d71\u7684\u300cNBR 70\u300d\u6a19\u7c64\u5247\u4e0d\u80fd\uff0c\u56e0\u70ba\u5b83\u5c0d\u6c7a\u5b9a\u8010\u6d41\u9ad4\u6027\u7684\u4e19\u70ef\u8148\u542b\u91cf\u96bb\u5b57\u4e0d\u63d0\u3002<\/p>\n<figure class=\"wp-block-image size-large\"><img decoding=\"async\" src=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/PU-HYDRAULIC-CYLINDER-WIPER-SEAL-DLI.png\" alt=\"\u805a\u6c28\u916f\u6db2\u58d3\u6cb9\u7f38\u9632\u5875\u5708DLI\u578b\u5ed3\" \/><figcaption>\u72c0\u6cc1\u826f\u597d\u7684 PU \u522e\u5875\u5708\uff1a\u4e00\u65e6\u5507\u908a\u7ff9\u8d77\u6216\u6495\u88c2\uff0c\u6c61\u57a2\u4fbf\u6703\u5230\u9054\u6d3b\u585e\u687f\u5bc6\u5c01\u4ef6\uff0c\u5931\u6548\u8a08\u6642\u96a8\u5373\u958b\u59cb<\/figcaption><\/figure>\n<h3>6. \u53d7\u6c61\u67d3\u6216\u52a3\u5316\u7684\u6d41\u9ad4<\/h3>\n<p>\u6cb9\u4e2d\u6c34\u5206\u8d85\u904e\u7d04 0.1% \u6703\u52a0\u901f\u6c27\u5316\u4e26\u524a\u5f31\u6f64\u6ed1\u6027\uff0c\u4ee4\u5bc6\u5c01\u4ef6\u5728\u6d3b\u585e\u687f\u4e0a\u4e7e\u78e8\u3002\u593e\u5e36\u7a7a\u6c23\u6703\u9020\u6210\u6c23\u8755\u640d\u58de\u53ca\u5c40\u90e8\u71b1\u9ede\u3002\u6c27\u5316\u6cb9\u6703\u5f62\u6210\u6f06\u819c\uff0c\u5c07\u5bc6\u5c01\u5507\u908a\u9ecf\u5728\u6d3b\u585e\u687f\u4e0a\uff0c\u4ee4\u505c\u6a5f\u5f8c\u7b2c\u4e00\u6b21\u884c\u7a0b\u6642\u5507\u908a\u6495\u88c2\u3002<\/p>\n<p>\u6b64\u539f\u56e0\u5f80\u5f80\u5728\u5bc6\u5c01\u4ef6\u672c\u8eab\u770b\u4e0d\u51fa\u4f86\u3002\u7dda\u7d22\u662f\u7cfb\u7d71\u5728\u4e00\u5e74\u5167\u65bc\u4e0d\u540c\u6cb9\u7f38\u51fa\u73fe\u4e09\u6b21\u5bc6\u5c01\u5931\u6548\uff0c\u4e14\u6c92\u6709\u5171\u540c\u7684\u5b89\u88dd\u932f\u8aa4\u3002\u5728\u7b2c\u56db\u6b21\u66f4\u63db\u4efb\u4f55\u6771\u897f\u4e4b\u524d\uff0c\u5148\u62bd\u53d6\u6d41\u9ad4\u6a23\u672c\u5316\u9a57\u3002<\/p>\n<h2>\u7b2c 3 \u7d44\uff1a\u6a5f\u68b0\u8ca0\u8f09\u8207\u8a2d\u8a08<\/h2>\n<h3>7. \u56e0\u9593\u9699\u904e\u5927\u800c\u88ab\u64e0\u51fa<\/h3>\n<p>\u7576\u58d3\u529b\u5c07\u5bc6\u5c01\u4ef6\u63a8\u5165\u6d3b\u585e\u687f\u8207\u58d3\u84cb\u4e4b\u9593\u7684\u9593\u9699\u6642\uff0c\u6750\u6599\u6703\u88ab\u526a\u5207\u6210\u8584\u7247\u3002\u7279\u5fb5\u975e\u5e38\u660e\u986f\uff1a\u640d\u58de\u96c6\u4e2d\u5728\u4f4e\u58d3\u908a\u7de3\uff0c\u5448\u6495\u88c2\u6216\u88ab\u5543\u54ac\u7684\u8f2a\u5ed3\uff0c\u800c\u975e\u78e8\u640d\u3002\u9019\u662f\u8a2d\u8a08\u6216\u78e8\u640d\u554f\u984c\uff0c\u4e0d\u662f\u6750\u6599\u554f\u984c\u3002<\/p>\n<figure class=\"wp-block-image size-large\"><img decoding=\"async\" src=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/SPG-piston-seal-double-acting.png\" alt=\"\u7528\u65bc\u6db2\u58d3\u6cb9\u7f38\u7684SPG\u96d9\u4f5c\u7528\u6d3b\u585e\u5bc6\u5c01\u4ef6\" \/><figcaption>\u96d9\u4f5c\u7528\u6d3b\u585e\u5bc6\u5c01\u4ef6\u5728\u5169\u9762\u4ea4\u66ff\u627f\u53d7\u58d3\u529b\uff0c\u56e0\u6b64\u5169\u5074\u7684\u9593\u9699\u63a7\u5236\u53ca\u64cb\u5708\u90fd\u5f88\u91cd\u8981<\/figcaption><\/figure>\n<p>\u5169\u7a2e\u4fee\u6b63\u65b9\u6cd5\u6709\u6548\u3002\u66f4\u63db\u6d3b\u585e\u687f\u896f\u5957\u6216\u5c0e\u5411\u74b0\u4ee5\u6536\u7dca\u9593\u9699\uff0c\u6216\u52a0\u88dd <a href=\"https:\/\/www.bosssealing.com\/zh\/what-is-a-backup-ring\/\">\u64cb\u5708<\/a> \u4ee5\u586b\u88dc\u9593\u9699\u3002\u7d04 160\u2013250 bar \u4ee5\u4e0a\uff0c\u64cb\u5708\u61c9\u5f9e\u4e00\u958b\u59cb\u5c31\u7d0d\u5165\u8a2d\u8a08\u3002\u82e5\u4f60\u5df2\u5728\u9032\u884c\u7ffb\u4fee\uff0c\u8f03\u4fbf\u5b9c\u7684\u7dad\u4fee\u5e7e\u4e4e\u7e3d\u662f\u52a0\u88dd\u64cb\u5708\u3002\u9019\u4e9b\u6578\u5b57\u80cc\u5f8c\u7684\u9593\u9699\u8868\u520a\u8f09\u65bc\u4ee5\u4e0b\u516c\u53f8\u7684\u5bc6\u5c01\u4ef6\u76ee\u9304\u4e2d\uff1a <a href=\"https:\/\/www.trelleborg.com\/en\/seals\/products-and-solutions\">Trelleborg<\/a>\uff0c\u5c07\u4f60\u7684\u58d3\u84cb\u8207\u5df2\u516c\u5e03\u7684\u8868\u683c\u6bd4\u8f03\u53ea\u9700\u5e7e\u5206\u9418\u3002<\/p>\n<h3>8. \u5074\u5411\u8ca0\u8f09\u8207\u4e0d\u5c0d\u4e2d<\/h3>\n<p>\u6d3b\u585e\u687f\u8207\u5176\u8ca0\u8f09\u4e0d\u540c\u5fc3\uff0c\u6703\u5c07\u6574\u500b\u5bc6\u5c01\u529b\u96c6\u4e2d\u65bc\u5507\u908a\u7684\u4e00\u6bb5\u5f27\u4e0a\u3002\u78e8\u640d\u5448\u6708\u7259\u5f62\u800c\u975e\u74b0\u5f62\uff0c\u6cb9\u7f38\u5728\u67d0\u4e00\u9418\u9ede\u4f4d\u7f6e\u6ef2\u6f0f\u3002\u539f\u56e0\u5305\u62ec\u6d3b\u585e\u687f\u8ef8\u627f\u78e8\u640d\u3001\u6d3b\u585e\u687f\u5f4e\u66f2\u3001\u6a5f\u67b6\u8b8a\u5f62\uff0c\u4ee5\u53ca\u672a\u5c0d\u6e96\u4fbf\u9396\u7dca\u7684\u5b89\u88dd\u87ba\u6813\u3002<\/p>\n<p>\u5728\u6574\u500b\u884c\u7a0b\u4e0a\u7528\u5343\u5206\u9336\u6aa2\u67e5\u6d3b\u585e\u687f\u7684\u504f\u64fa\u3002\u6bcf\u7c73\u504f\u5dee\u8d85\u904e\u7d04 0.05 mm \u4fbf\u8db3\u4ee5\u4ee4\u9577\u884c\u7a0b\u6cb9\u7f38\u7684\u5bc6\u5c01\u58fd\u547d\u6e1b\u534a\u3002\u4efb\u4f55\u5bc6\u5c01\u8f2a\u5ed3\u90fd\u7121\u6cd5\u88dc\u511f\u5074\u5411\u8ca0\u8f09\uff1b\u6821\u6b63\u5c0d\u6e96\u5247\u53ef\u4ee5\u3002<\/p>\n<h3>9. \u58d3\u529b\u5c16\u5cf0\u8207\u885d\u64ca\u8ca0\u8f09<\/h3>\n<p>\u984d\u5b9a 200 bar \u7684\u7cfb\u7d71\uff0c\u7576\u95a5\u9580\u5728\u8ca0\u8f09\u79fb\u52d5\u6642\u95dc\u9589\uff0c\u53ef\u5728\u6578\u6beb\u79d2\u5167\u9054\u5230 350 bar\u3002\u9019\u4e9b\u5c16\u5cf0\u6703\u64e0\u51fa\u5b8c\u5168\u7b26\u5408\u7a69\u614b\u58d3\u529b\u984d\u5b9a\u7684\u5bc6\u5c01\u4ef6\uff0c\u4e26\u4f7f\u5f48\u6027\u9ad4\u75b2\u52de\u76f4\u81f3\u9f9c\u88c2\u3002\u8b49\u64da\u662f\u5bc6\u5c01\u4ef6\u63d0\u65e9\u5931\u6548\uff0c\u908a\u7de3\u8106\u5f31\u788e\u88c2\uff0c\u5b8c\u5168\u6c92\u6709\u78e8\u640d\u6a21\u5f0f\u3002<\/p>\n<p>\u6aa2\u67e5\u6d29\u58d3\u95a5\u662f\u5426\u8a2d\u5b9a\u904e\u9ad8\u6216\u53cd\u61c9\u904e\u6162\u3001\u84c4\u80fd\u5668\u662f\u5426\u5931\u53bb\u9810\u5145\u58d3\u529b\uff0c\u4ee5\u53ca\u95a5\u9580\u5207\u63db\u6642\u9593\u662f\u5426\u5feb\u65bc\u7cfb\u7d71\u6240\u80fd\u5438\u6536\u3002\u52a0\u88dd\u7de9\u885d\u6216\u6e1b\u6162\u6ed1\u95a5\u7684\u901f\u5ea6\uff0c\u6210\u672c\u4f4e\u65bc\u5176\u6240\u80fd\u907f\u514d\u7684\u5bc6\u5c01\u4ef6\u66f4\u63db\u3002<\/p>\n<h3>10. \u5b89\u88dd\u640d\u58de\u8207\u932f\u8aa4\u7d44\u88dd<\/h3>\n<p>\u87ba\u65cb\u7d0b\u6a6b\u904e\u5507\u53e3\u3001\u5507\u53e3\u5411\u5916\u7ffb\u6372\u3001\u5bc6\u5c01\u4ef6\u5728\u6c92\u6709\u5957\u7b52\u7684\u60c5\u6cc1\u4e0b\u88ab\u62c9\u4f38\u5957\u4e0a\u87ba\u7d0b\u687f\u7aef\uff0c\u6216\u7528\u87ba\u7d72\u6279\u5f37\u884c\u58d3\u5165\u5bc6\u5c01\u4ef6\uff1a\u9019\u4e9b\u90fd\u6703\u7559\u4e0b\u770b\u4f3c\u88fd\u9020\u7f3a\u9677\u3001\u4f46\u5be6\u969b\u4e0a\u4e26\u975e\u7f3a\u9677\u7684\u75d5\u8de1\u3002\u5b89\u88dd\u6642\u53d7\u640d\u7684\u5bc6\u5c01\u4ef6\uff0c\u901a\u5e38\u6703\u5728\u6578\u5c0f\u6642\u81f3\u6578\u65e5\u5167\u5931\u6548\u3002<\/p>\n<p>\u4e09\u500b\u7fd2\u6163\u53ef\u907f\u514d\u6b64\u60c5\u6cc1\uff1a\u7528\u81a0\u5e36\u6216\u5c0e\u5165\u5957\u84cb\u4f4f\u87ba\u7d0b\u53ca\u82b1\u9375\u3001\u4ee5\u6f54\u6de8\u7684\u7cfb\u7d71\u6d41\u9ad4\u6f64\u6ed1\uff0c\u4e26\u5728\u5408\u4e0a\u58d3\u84cb\u524d\u7528\u624b\u611f\u89ba\u78ba\u8a8d\u5507\u53e3\u5df2\u6cbf\u6574\u500b\u5713\u5468\u5c31\u4f4d\u3002\u82e5\u6cb9\u7f38\u5728\u7ffb\u4fee\u5f8c\u7acb\u5373\u6ef2\u6f0f\uff0c\u61c9\u5148\u5047\u8a2d\u662f\u5b89\u88dd\u640d\u50b7\uff0c\u800c\u975e\u5047\u8a2d\u96f6\u4ef6\u6709\u554f\u984c\u3002<\/p>\n<h2>\u627e\u51fa\u6210\u56e0\u768430\u5206\u9418\u6aa2\u67e5<\/h2>\n<p>\u7576\u5bc6\u5c01\u4ef6\u63d0\u65e9\u5931\u6548\u6642\uff0c\u5728\u8a02\u8cfc\u66ff\u63db\u4ef6\u524d\u5148\u82b1\u534a\u5c0f\u6642\u3002\u4ee5\u4e0b\u6b65\u9a5f\u5728\u5927\u591a\u6578\u60c5\u6cc1\u4e0b\u80fd\u627e\u51fa\u6210\u56e0\uff0c\u9664\u5361\u5c3a\u3001\u5343\u5206\u9336\u53ca\u6a23\u672c\u74f6\u5916\u7121\u9700\u7279\u6b8a\u5de5\u5177\u3002<\/p>\n<table>\n<thead>\n<tr>\n<th>\u6b65\u9a5f<\/th>\n<th>\u8981\u505a\u7684\u4e8b<\/th>\n<th>\u53ef\u6392\u9664\u7684\u539f\u56e0<\/th>\n<\/tr>\n<\/thead>\n<tbody>\n<tr>\n<td>1<\/td>\n<td>\u5728\u6e05\u6f54\u524d\uff0c\u5148\u62cd\u651d\u5bc6\u5c01\u4ef6\u5728\u539f\u4f4d\u53ca\u62c6\u4e0b\u5f8c\u7684\u7167\u7247<\/td>\n<td>\u4e0d\u6703\u56e0\u8655\u7406\u800c\u6d41\u5931\u8b49\u64da<\/td>\n<\/tr>\n<tr>\n<td>2<\/td>\n<td>\u91cf\u5ea6\u622a\u9762\u4e26\u8207\u65b0\u4ef6\u6bd4\u8f03\uff0c\u8a18\u9304\u81a8\u8139\u6216\u6536\u7e2e<\/td>\n<td>\u5316\u5b78\u4e0d\u76f8\u5bb9\u3001\u58d3\u7e2e\u6c38\u4e45\u8b8a\u5f62<\/td>\n<\/tr>\n<tr>\n<td>3<\/td>\n<td>\u6aa2\u67e5\u5507\u53e3\u662f\u5543\u8755\u3001\u5747\u52fb\u78e8\u640d\u9084\u662f\u5272\u50b7<\/td>\n<td>\u64e0\u51fa\u3001\u6b63\u5e38\u58fd\u547d\u3001\u5b89\u88dd\u640d\u50b7<\/td>\n<\/tr>\n<tr>\n<td>4<\/td>\n<td>\u91cf\u5ea6\u58d3\u84cb\u9593\u9699\u53ca\u6e9d\u69fd\u6df1\u5ea6<\/td>\n<td>\u64e0\u51fa\u3001\u904e\u5ea6\u58d3\u7e2e<\/td>\n<\/tr>\n<tr>\n<td>5<\/td>\n<td>\u7528\u5343\u5206\u9336\u6aa2\u67e5\u6d3b\u585e\u687f\u5728\u6574\u500b\u884c\u7a0b\u7684\u504f\u64fa<\/td>\n<td>\u5074\u5411\u8ca0\u8f09\u53ca\u4e0d\u5c0d\u4e2d<\/td>\n<\/tr>\n<tr>\n<td>6<\/td>\n<td>\u6aa2\u67e5\u9632\u5875\u5708\u53ca\u547c\u5438\u5668\u7684\u72c0\u6cc1<\/td>\n<td>\u5916\u4f86\u6c61\u67d3\u7269\u4fb5\u5165<\/td>\n<\/tr>\n<tr>\n<td>7<\/td>\n<td>\u62bd\u53d6\u6cb9\u6a23\u672c\u5316\u9a57\u9846\u7c92\u8a08\u6578\u53ca\u542b\u6c34\u91cf<\/td>\n<td>\u6d41\u9ad4\u52a3\u5316\u3001\u78e8\u8755\u6027\u6c61\u67d3<\/td>\n<\/tr>\n<tr>\n<td>8<\/td>\n<td>\u8a18\u9304\u6cb9\u7f38\u5728\u8ca0\u8f09\u4e0b\u7684\u6d41\u9ad4\u6eab\u5ea6<\/td>\n<td>\u6eab\u5ea6\u904e\u9ad8<\/td>\n<\/tr>\n<\/tbody>\n<\/table>\n<p>\u6839\u64da\u6211\u5011\u7684\u7d93\u9a57\uff0c\u55ae\u662f\u6b65\u9a5f3\u5df2\u80fd\u5728\u7d04\u5341\u500b\u500b\u6848\u4e2d\u7684\u4e03\u500b\u627e\u51fa\u6210\u56e0\u3002\u6b65\u9a5f4\u81f36\u5247\u544a\u8a34\u4f60\u89e3\u6c7a\u65b9\u6cd5\u662f\u63db\u96f6\u4ef6\u3001\u7dad\u4fee\u9084\u662f\u6539\u8b8a\u7a0b\u5e8f\u3002<\/p>\n<h2>\u91cd\u9ede\u6458\u8981<\/h2>\n<ul>\n<li>\u5728\u8a02\u8cfc\u66ff\u63db\u4ef6\u524d\u5148\u8b80\u61c2\u640d\u50b7\u6a21\u5f0f\u3002\u5507\u53e3\u7684\u5916\u89c0\u6bd4\u4efb\u4f55\u6578\u64da\u8868\u90fd\u66f4\u80fd\u5feb\u901f\u6536\u7a84\u6210\u56e0\u3002<\/li>\n<li>\u6c61\u67d3\u800c\u975e\u6750\u6599\u54c1\u8cea\uff0c\u662f\u6700\u5e38\u898b\u7684\u6839\u672c\u539f\u56e0\uff0c\u800c\u9632\u5875\u5708\u6b63\u662f\u8b93\u6c61\u67d3\u9032\u5165\u7684\u96f6\u4ef6\u3002<\/li>\n<li>\u908a\u7de3\u5543\u8755\u4ee3\u8868\u64e0\u51fa\uff1a\u6aa2\u67e5\u9593\u9699\u4e26\u88dd\u4e0a\u64cb\u5708\uff0c\u800c\u975e\u6539\u7528\u66f4\u786c\u7684\u81a0\u6599\u3002<\/li>\n<li>\u65b0\u6708\u5f62\u78e8\u640d\u4ee3\u8868\u5074\u5411\u8ca0\u8f09\u3002\u66f4\u63db\u5c0e\u5411\u5143\u4ef6\u6216\u6821\u6b63\u5c0d\u4e2d\uff1b\u5bc6\u5c01\u4ef6\u53ea\u662f\u75c7\u72c0\u3002<\/li>\n<li>\u5507\u53e3\u786c\u5316\u3001\u9f9c\u88c2\u4ee3\u8868\u9ad8\u6eab\uff0c\u800c\u6eab\u5ea6\u61c9\u5728\u58d3\u84cb\u8655\u91cf\u5ea6\uff0c\u800c\u975e\u5728\u6cb9\u7bb1\u8655\u3002<\/li>\n<li>\u7ffb\u4fee\u5f8c\u6578\u65e5\u5167\u5931\u6548\u7684\u5bc6\u5c01\u4ef6\uff0c\u5e7e\u4e4e\u53ef\u4ee5\u80af\u5b9a\u662f\u5728\u5b89\u88dd\u671f\u9593\u53d7\u640d\u3002<\/li>\n<li>\u4e00\u5e74\u5167\u5728\u4e0d\u540c\u6cb9\u7f38\u51fa\u73fe\u4e09\u6b21\u5931\u6548\uff0c\u6307\u5411\u6d41\u9ad4\u554f\u984c\uff0c\u800c\u975e\u5bc6\u5c01\u4ef6\u554f\u984c\u3002<\/li>\n<\/ul>\n<p>\u82e5\u6aa2\u67e5\u5f8c\u6210\u56e0\u4ecd\u4e0d\u660e\u78ba\uff0c\u8acb\u628a\u5931\u6548\u7684\u5bc6\u5c01\u4ef6\u3001\u58d3\u84cb\u5c3a\u5bf8\u53ca\u6d41\u9ad4\u6578\u64da\u5bc4\u7d66\u6211\u5011\u3002\u6211\u5011\u7684 <a href=\"https:\/\/www.bosssealing.com\/zh\/%e7%94%a2%e5%93%81%e5%88%86%e9%a1%9e\/%e6%b6%b2%e5%a3%93%e6%a1%bf%e5%af%86%e5%b0%81%e4%bb%b6\/\">\u6d3b\u585e\u687f\u5bc6\u5c01\u4ef6\u7cfb\u5217<\/a> \u53ca <a href=\"https:\/\/www.bosssealing.com\/zh\/%e7%94%a2%e5%93%81%e5%88%86%e9%a1%9e\/%e9%ab%98%e6%ba%ab%e4%bd%8e%e6%ba%ab%e5%af%86%e5%b0%81%e4%bb%b6\/\">\u9ad8\u4f4e\u6eab\u5bc6\u5c01\u4ef6\u7cfb\u5217<\/a> \u6db5\u84cb\u6700\u5e38\u6d89\u53ca\u7684\u578b\u5ed3\uff0c\u800c\u91dd\u5c0d\u6709\u95dc\u6cb9\u7f38\u7684\u7ffb\u4fee\u5957\u4ef6\u901a\u5e38\u5728\u6839\u672c\u539f\u56e0\u7cfe\u6b63\u5f8c\u80fd\u6c38\u4e45\u89e3\u6c7a\u554f\u984c\u3002 <a href=\"https:\/\/www.bosssealing.com\/zh\/hydraulic-cylinder-seal-kit-guide\/\">\u6cb9\u7f38\u5bc6\u5c01\u4ef6\u5957\u4ef6\u6307\u5357<\/a> \u8aaa\u660e\u5982\u4f55\u6307\u5b9a\u6574\u5957\u5bc6\u5c01\u4ef6\uff0c\u4ee5\u514d\u4e00\u500b\u78e8\u640d\u7684\u9632\u5875\u5708\u5728\u516d\u500b\u6708\u5f8c\u6f14\u8b8a\u6210\u7b2c\u4e8c\u6b21\u7ffb\u4fee\u3002<\/p>","protected":false},"excerpt":{"rendered":"<p>\u5f9e\u640d\u58de\u5f62\u614b\u8a3a\u65b7\u6db2\u58d3\u5bc6\u5c01\u4ef6\u5931\u6548\uff1a\u5341\u7a2e\u539f\u56e0\u53ca\u5176\u8996\u89ba\u7279\u5fb5\u3001\u5206\u7d44\u6aa2\u67e5\uff0c\u4ee5\u53ca30\u5206\u9418\u6aa2\u67e5\u6d41\u7a0b\u3002<\/p>","protected":false},"author":1,"featured_media":1646,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_monsterinsights_skip_tracking":false,"footnotes":""},"categories":[1],"tags":[],"class_list":["post-1649","post","type-post","status-publish","format-standard","has-post-thumbnail","hentry","category-news"],"aioseo_notices":[],"aioseo_head":"\n\t\t<!-- All in One SEO 5.0.4 - aioseo.com -->\n\t<meta name=\"description\" content=\"The 10 most common hydraulic seal failure causes with their visual signatures: extrusion, heat, contamination, side load, plus a 30-minute diagnostic.\" \/>\n\t<meta name=\"robots\" content=\"max-image-preview:large\" \/>\n\t<meta name=\"author\" content=\"boss\"\/>\n\t<link rel=\"canonical\" href=\"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/\" \/>\n\t\t<meta name=\"generator\" content=\"All in One SEO (AIOSEO) 5.0.4\" \/>\n\t\t<meta property=\"og:locale\" content=\"zh_HK\" \/>\n\t\t<meta property=\"og:site_name\" content=\"BOSS Sealing Solutions - Hydraulic seal and pneumatic seal factory\" \/>\n\t\t<meta property=\"og:type\" content=\"article\" \/>\n\t\t<meta property=\"og:title\" content=\"Top 10 Causes of Hydraulic Seal Failure (and the Fixes)\" \/>\n\t\t<meta property=\"og:description\" content=\"The 10 most common hydraulic seal failure causes with their visual signatures: extrusion, heat, contamination, side load, plus a 30-minute diagnostic.\" \/>\n\t\t<meta property=\"og:url\" content=\"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/\" \/>\n\t\t<meta property=\"og:image\" content=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png\" \/>\n\t\t<meta property=\"og:image:secure_url\" content=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png\" \/>\n\t\t<meta property=\"article:published_time\" content=\"2026-11-03T12:43:00+00:00\" \/>\n\t\t<meta property=\"article:modified_time\" content=\"2026-11-03T12:43:00+00:00\" \/>\n\t\t<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n\t\t<meta name=\"twitter:title\" content=\"Top 10 Causes of Hydraulic Seal Failure (and the Fixes)\" \/>\n\t\t<meta name=\"twitter:description\" content=\"The 10 most common hydraulic seal failure causes with their visual signatures: extrusion, heat, contamination, side load, plus a 30-minute diagnostic.\" \/>\n\t\t<meta name=\"twitter:image\" content=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png\" \/>\n\t\t<script type=\"application\/ld+json\" class=\"aioseo-schema\">\n\t\t\t{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"BlogPosting\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#blogposting\",\"name\":\"Top 10 Causes of Hydraulic Seal Failure (and the Fixes)\",\"headline\":\"Top 10 Causes of Hydraulic Seal Failure and How to Prevent Each One\",\"author\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/#author\"},\"publisher\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#organization\"},\"image\":{\"@type\":\"ImageObject\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/wp-content\\\/uploads\\\/2026\\\/11\\\/rod_seal_failure.jpg\",\"width\":1536,\"height\":944,\"caption\":\"Failed polyurethane hydraulic rod seal with a torn lip next to a caliper and worn chrome rod\"},\"datePublished\":\"2026-11-03T20:43:00+08:00\",\"dateModified\":\"2026-11-03T20:43:00+08:00\",\"inLanguage\":\"zh-HK\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#webpage\"},\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#webpage\"},\"articleSection\":\"Knowledge Base\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#breadcrumblist\",\"itemListElement\":[{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#listItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/\",\"nextItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/category\\\/news\\\/#listItem\",\"name\":\"Knowledge Base\"}},{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/category\\\/news\\\/#listItem\",\"position\":2,\"name\":\"Knowledge Base\",\"item\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/category\\\/news\\\/\",\"nextItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#listItem\",\"name\":\"Top 10 Causes of Hydraulic Seal Failure and How to Prevent Each One\"},\"previousItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#listItem\",\"name\":\"Home\"}},{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#listItem\",\"position\":3,\"name\":\"Top 10 Causes of Hydraulic Seal Failure and How to Prevent Each One\",\"previousItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/category\\\/news\\\/#listItem\",\"name\":\"Knowledge Base\"}}]},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#organization\",\"name\":\"BOSS Sealing Solutions\",\"description\":\"Hydraulic seal and pneumatic seal factory\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/\",\"email\":\"sales@bosssealing.com\",\"telephone\":\"+86 13392768056\",\"logo\":{\"@type\":\"ImageObject\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/wp-content\\\/uploads\\\/2023\\\/07\\\/logo.png\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#organizationLogo\",\"width\":1744,\"height\":555,\"caption\":\"BOSS Sealing Solutions\"},\"image\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#organizationLogo\"}},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/#author\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/\",\"name\":\"boss\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#webpage\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/\",\"name\":\"Top 10 Causes of Hydraulic Seal Failure (and the Fixes)\",\"description\":\"The 10 most common hydraulic seal failure causes with their visual signatures: extrusion, heat, contamination, side load, plus a 30-minute diagnostic.\",\"inLanguage\":\"zh-HK\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#website\"},\"breadcrumb\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#breadcrumblist\"},\"author\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/#author\"},\"creator\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/author\\\/boss\\\/#author\"},\"image\":{\"@type\":\"ImageObject\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/wp-content\\\/uploads\\\/2026\\\/11\\\/rod_seal_failure.jpg\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#mainImage\",\"width\":1536,\"height\":944,\"caption\":\"Failed polyurethane hydraulic rod seal with a torn lip next to a caliper and worn chrome rod\"},\"primaryImageOfPage\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/hydraulic-seal-failure-causes\\\/#mainImage\"},\"datePublished\":\"2026-11-03T20:43:00+08:00\",\"dateModified\":\"2026-11-03T20:43:00+08:00\"},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#website\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/\",\"name\":\"BOSS Sealing Solutions\",\"alternateName\":\"BOSS Sealing\",\"description\":\"Hydraulic seal and pneumatic seal factory\",\"inLanguage\":\"zh-HK\",\"publisher\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/zh\\\/#organization\"}}]}\n\t\t<\/script>\n\t\t<!-- All in One SEO -->\n\n","aioseo_head_json":{"title":"\u6db2\u58d3\u5bc6\u5c01\u4ef6\u5931\u6548\u7684\u5341\u5927\u539f\u56e0\uff08\u4ee5\u53ca\u89e3\u6c7a\u65b9\u6cd5\uff09","description":"\u6700\u5e38\u898b\u560510\u500b\u6db2\u58d3\u5bc6\u5c01\u4ef6\u5931\u6548\u539f\u56e0\u540c\u57cb\u4f62\u54cb\u5605\u5916\u89c0\u7279\u5fb5\uff1a\u64e0\u51fa\u3001\u904e\u71b1\u3001\u6c61\u67d3\u3001\u5074\u5411\u8ca0\u8f09\uff0c\u53e6\u5916\u4ef2\u6709\u4e00\u500b30\u5206\u9418\u5605\u8a3a\u65b7\u3002","canonical_url":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/","robots":"max-image-preview:large","keywords":"","webmasterTools":{"miscellaneous":""},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"BlogPosting","@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#blogposting","name":"Top 10 Causes of Hydraulic Seal Failure (and the Fixes)","headline":"Top 10 Causes of Hydraulic Seal Failure and How to Prevent Each One","author":{"@id":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/#author"},"publisher":{"@id":"https:\/\/www.bosssealing.com\/zh\/#organization"},"image":{"@type":"ImageObject","url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2026\/11\/rod_seal_failure.jpg","width":1536,"height":944,"caption":"Failed polyurethane hydraulic rod seal with a torn lip next to a caliper and worn chrome rod"},"datePublished":"2026-11-03T20:43:00+08:00","dateModified":"2026-11-03T20:43:00+08:00","inLanguage":"zh-HK","mainEntityOfPage":{"@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#webpage"},"isPartOf":{"@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#webpage"},"articleSection":"Knowledge Base"},{"@type":"BreadcrumbList","@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#breadcrumblist","itemListElement":[{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/#listItem","position":1,"name":"Home","item":"https:\/\/www.bosssealing.com\/zh\/","nextItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/category\/news\/#listItem","name":"Knowledge Base"}},{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/category\/news\/#listItem","position":2,"name":"Knowledge Base","item":"https:\/\/www.bosssealing.com\/zh\/category\/news\/","nextItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#listItem","name":"Top 10 Causes of Hydraulic Seal Failure and How to Prevent Each One"},"previousItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/#listItem","name":"Home"}},{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#listItem","position":3,"name":"Top 10 Causes of Hydraulic Seal Failure and How to Prevent Each One","previousItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/zh\/category\/news\/#listItem","name":"Knowledge Base"}}]},{"@type":"Organization","@id":"https:\/\/www.bosssealing.com\/zh\/#organization","name":"BOSS Sealing Solutions","description":"Hydraulic seal and pneumatic seal factory","url":"https:\/\/www.bosssealing.com\/zh\/","email":"sales@bosssealing.com","telephone":"+86 13392768056","logo":{"@type":"ImageObject","url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#organizationLogo","width":1744,"height":555,"caption":"BOSS Sealing Solutions"},"image":{"@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#organizationLogo"}},{"@type":"Person","@id":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/#author","url":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/","name":"boss"},{"@type":"WebPage","@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#webpage","url":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/","name":"Top 10 Causes of Hydraulic Seal Failure (and the Fixes)","description":"The 10 most common hydraulic seal failure causes with their visual signatures: extrusion, heat, contamination, side load, plus a 30-minute diagnostic.","inLanguage":"zh-HK","isPartOf":{"@id":"https:\/\/www.bosssealing.com\/zh\/#website"},"breadcrumb":{"@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#breadcrumblist"},"author":{"@id":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/#author"},"creator":{"@id":"https:\/\/www.bosssealing.com\/zh\/author\/boss\/#author"},"image":{"@type":"ImageObject","url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2026\/11\/rod_seal_failure.jpg","@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#mainImage","width":1536,"height":944,"caption":"Failed polyurethane hydraulic rod seal with a torn lip next to a caliper and worn chrome rod"},"primaryImageOfPage":{"@id":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/#mainImage"},"datePublished":"2026-11-03T20:43:00+08:00","dateModified":"2026-11-03T20:43:00+08:00"},{"@type":"WebSite","@id":"https:\/\/www.bosssealing.com\/zh\/#website","url":"https:\/\/www.bosssealing.com\/zh\/","name":"BOSS Sealing Solutions","alternateName":"BOSS Sealing","description":"Hydraulic seal and pneumatic seal factory","inLanguage":"zh-HK","publisher":{"@id":"https:\/\/www.bosssealing.com\/zh\/#organization"}}]},"og:locale":"zh_HK","og:site_name":"BOSS Sealing Solutions - Hydraulic seal and pneumatic seal factory","og:type":"article","og:title":"Top 10 Causes of Hydraulic Seal Failure (and the Fixes)","og:description":"The 10 most common hydraulic seal failure causes with their visual signatures: extrusion, heat, contamination, side load, plus a 30-minute diagnostic.","og:url":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/","og:image":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","og:image:secure_url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","article:published_time":"2026-11-03T12:43:00+00:00","article:modified_time":"2026-11-03T12:43:00+00:00","twitter:card":"summary_large_image","twitter:title":"Top 10 Causes of Hydraulic Seal Failure (and the Fixes)","twitter:description":"The 10 most common hydraulic seal failure causes with their visual signatures: extrusion, heat, contamination, side load, plus a 30-minute diagnostic.","twitter:image":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png"},"aioseo_meta_data":{"post_id":"1649","title":"\u6db2\u58d3\u5bc6\u5c01\u4ef6\u5931\u6548\u7684\u5341\u5927\u539f\u56e0\uff08\u4ee5\u53ca\u89e3\u6c7a\u65b9\u6cd5\uff09","description":"\u6700\u5e38\u898b\u560510\u500b\u6db2\u58d3\u5bc6\u5c01\u4ef6\u5931\u6548\u539f\u56e0\u540c\u57cb\u4f62\u54cb\u5605\u5916\u89c0\u7279\u5fb5\uff1a\u64e0\u51fa\u3001\u904e\u71b1\u3001\u6c61\u67d3\u3001\u5074\u5411\u8ca0\u8f09\uff0c\u53e6\u5916\u4ef2\u6709\u4e00\u500b30\u5206\u9418\u5605\u8a3a\u65b7\u3002","keywords":null,"keyphrases":{"focus":[],"additional":[]},"primary_term":null,"canonical_url":null,"og_title":null,"og_description":null,"og_object_type":"default","og_image_type":"default","og_image_url":null,"og_image_width":null,"og_image_height":null,"og_image_custom_url":null,"og_image_custom_fields":null,"og_video":"","og_custom_url":null,"og_article_section":null,"og_article_tags":null,"twitter_use_og":false,"twitter_card":"default","twitter_image_type":"default","twitter_image_url":null,"twitter_image_custom_url":null,"twitter_image_custom_fields":null,"twitter_title":null,"twitter_description":null,"schema":{"blockGraphs":[],"customGraphs":[],"default":{"data":{"Article":[],"Course":[],"Dataset":[],"FAQPage":[],"Movie":[],"Person":[],"Product":[],"ProductReview":[],"Car":[],"Recipe":[],"Service":[],"SoftwareApplication":[],"WebPage":[]},"graphName":"BlogPosting","isEnabled":true},"graphs":[]},"schema_type":"default","schema_type_options":null,"pillar_content":false,"robots_default":true,"robots_noindex":false,"robots_noarchive":false,"robots_nosnippet":false,"robots_nofollow":false,"robots_noimageindex":false,"robots_noodp":false,"robots_notranslate":false,"robots_max_snippet":"-1","robots_max_videopreview":"-1","robots_max_imagepreview":"large","priority":null,"frequency":"default","local_seo":null,"breadcrumb_settings":null,"limit_modified_date":false,"ai":{"faqs":[],"keyPoints":[],"schemas":[],"titles":[],"descriptions":[],"socialPosts":{"email":[],"linkedin":[],"twitter":[],"facebook":[],"instagram":[]}},"created":"2026-11-02 09:06:40","updated":"2026-11-03 13:01:56","seo_analyzer_scan_date":null,"focus_keyword":null,"additional_keywords":null,"truseo_locale":null},"aioseo_breadcrumb":"<div class=\"aioseo-breadcrumbs\"><span class=\"aioseo-breadcrumb\">\n\t\t\t<a href=\"https:\/\/www.bosssealing.com\/zh\/\" title=\"Home\">Home<\/a>\n\t\t<\/span><span class=\"aioseo-breadcrumb-separator\">\u00bb<\/span><span class=\"aioseo-breadcrumb\">\n\t\t\t<a href=\"https:\/\/www.bosssealing.com\/zh\/category\/news\/\" title=\"Knowledge Base\">Knowledge Base<\/a>\n\t\t<\/span><span class=\"aioseo-breadcrumb-separator\">\u00bb<\/span><span class=\"aioseo-breadcrumb\">\n\t\t\tTop 10 Causes of Hydraulic Seal Failure and How to Prevent Each One\n\t\t<\/span><\/div>","aioseo_breadcrumb_json":[{"label":"Home","link":"https:\/\/www.bosssealing.com\/zh\/"},{"label":"Knowledge Base","link":"https:\/\/www.bosssealing.com\/zh\/category\/news\/"},{"label":"Top 10 Causes of Hydraulic Seal Failure and How to Prevent Each One","link":"https:\/\/www.bosssealing.com\/zh\/hydraulic-seal-failure-causes\/"}],"_links":{"self":[{"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/posts\/1649","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/comments?post=1649"}],"version-history":[{"count":1,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/posts\/1649\/revisions"}],"predecessor-version":[{"id":1665,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/posts\/1649\/revisions\/1665"}],"wp:featuredmedia":[{"embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/media\/1646"}],"wp:attachment":[{"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/media?parent=1649"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/categories?post=1649"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.bosssealing.com\/zh\/wp-json\/wp\/v2\/tags?post=1649"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}