{"id":218,"date":"2021-06-09T11:09:36","date_gmt":"2021-06-09T03:09:36","guid":{"rendered":"https:\/\/boss.xgtu.cn\/fep-manufacturing-process\/"},"modified":"2023-07-18T14:18:30","modified_gmt":"2023-07-18T06:18:30","slug":"%d0%bf%d1%80%d0%be%d1%86%d0%b5%d1%81%d1%81-%d0%bf%d1%80%d0%be%d0%b8%d0%b7%d0%b2%d0%be%d0%b4%d1%81%d1%82%d0%b2%d0%b0-fep","status":"publish","type":"post","link":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/","title":{"rendered":"\u041f\u0440\u043e\u0446\u0435\u0441\u0441 \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0430 FEP"},"content":{"rendered":"<div class=\"contents\">\n<h1 class=\"contents_title\">\u041f\u0440\u043e\u0446\u0435\u0441\u0441 \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0430 FEP<\/h1>\n<p>\u041f\u0440\u043e\u0446\u0435\u0441\u0441 \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0430 FEP<\/p>\n<p>FEP \u043e\u0431\u043b\u0430\u0434\u0430\u0435\u0442 \u043b\u0443\u0447\u0448\u0438\u043c\u0438 \u0442\u0435\u0445\u043d\u043e\u043b\u043e\u0433\u0438\u0447\u0435\u0441\u043a\u0438\u043c\u0438 \u0445\u0430\u0440\u0430\u043a\u0442\u0435\u0440\u0438\u0441\u0442\u0438\u043a\u0430\u043c\u0438. \u041d\u0438\u0436\u0435 \u043f\u0435\u0440\u0435\u0447\u0438\u0441\u043b\u0435\u043d\u043e \u0442\u043e, \u0447\u0442\u043e \u043d\u0435\u043e\u0431\u0445\u043e\u0434\u0438\u043c\u043e \u043f\u043e\u0434\u0433\u043e\u0442\u043e\u0432\u0438\u0442\u044c \u043f\u0435\u0440\u0435\u0434 \u044d\u043a\u0441\u0442\u0440\u0443\u0437\u0438\u0435\u0439 \u0442\u0440\u0443\u0431\u044b \u0438\u0437 FEP:<\/p>\n<p>1) \u041f\u043e\u0434\u0430\u0447\u0430: \u043f\u0435\u0440\u0435\u0434 \u044d\u043a\u0441\u0442\u0440\u0443\u0437\u0438\u0435\u0439 FEP \u043f\u0440\u0435\u0434\u0432\u0430\u0440\u0438\u0442\u0435\u043b\u044c\u043d\u043e \u043f\u0440\u043e\u043a\u0430\u043b\u0438\u0442\u0435 \u043f\u0440\u0438 120 \u2103 \u0432 \u0442\u0435\u0447\u0435\u043d\u0438\u0435 \u043f\u0440\u0438\u043c\u0435\u0440\u043d\u043e 3 \u0447.<\/p>\n<p>2) \u041f\u0440\u0435\u0434\u0432\u0430\u0440\u0438\u0442\u0435\u043b\u044c\u043d\u044b\u0439 \u043d\u0430\u0433\u0440\u0435\u0432 \u0442\u043e\u043a\u043e\u043f\u0440\u043e\u0432\u043e\u0434\u044f\u0449\u0435\u0439 \u0436\u0438\u043b\u044b: \u0447\u0442\u043e\u0431\u044b \u043e\u0431\u0435\u0441\u043f\u0435\u0447\u0438\u0442\u044c \u0440\u0430\u0432\u043d\u043e\u043c\u0435\u0440\u043d\u0443\u044e \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0443 \u0432\u043d\u0443\u0442\u0440\u0438 \u0438 \u0441\u043d\u0430\u0440\u0443\u0436\u0438 \u044d\u043a\u0441\u0442\u0440\u0443\u0434\u0438\u0440\u043e\u0432\u0430\u043d\u043d\u043e\u0433\u043e \u0438\u0437\u043e\u043b\u044f\u0446\u0438\u043e\u043d\u043d\u043e\u0433\u043e \u0441\u043b\u043e\u044f FEP, \u0442\u043e\u043a\u043e\u043f\u0440\u043e\u0432\u043e\u0434\u044f\u0449\u0443\u044e \u0436\u0438\u043b\u0443 \u0441\u043b\u0435\u0434\u0443\u0435\u0442 \u043f\u0440\u0435\u0434\u0432\u0430\u0440\u0438\u0442\u0435\u043b\u044c\u043d\u043e \u043d\u0430\u0433\u0440\u0435\u0442\u044c \u0434\u043e 300\u2013350 \u2103.<\/p>\n<p>3) \u0420\u0430\u0441\u043f\u0440\u0435\u0434\u0435\u043b\u0435\u043d\u0438\u0435 \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u044b \u043f\u043e \u0437\u043e\u043d\u0430\u043c \u044d\u043a\u0441\u0442\u0440\u0443\u0434\u0435\u0440\u0430: \u043a\u0430\u043a \u043f\u0440\u0430\u0432\u0438\u043b\u043e, \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0430 \u043f\u043e \u0437\u043e\u043d\u0430\u043c \u044d\u043a\u0441\u0442\u0440\u0443\u0434\u0435\u0440\u0430 \u043e\u0442 280 \u00b0C (\u0437\u0430\u0433\u0440\u0443\u0437\u043e\u0447\u043d\u043e\u0435 \u043e\u0442\u0432\u0435\u0440\u0441\u0442\u0438\u0435) \u0434\u043e 380 \u00b0C (\u0433\u043e\u043b\u043e\u0432\u043a\u0430) \u043f\u043e\u0432\u044b\u0448\u0430\u0435\u0442\u0441\u044f \u043b\u0438\u043d\u0435\u0439\u043d\u043e;<\/p>\n<p>4) \u0421\u0442\u0435\u043f\u0435\u043d\u044c \u0432\u044b\u0442\u044f\u0436\u043a\u0438 \u043c\u0430\u0442\u0440\u0438\u0447\u043d\u043e\u0439 \u0432\u0442\u0443\u043b\u043a\u0438: \u0441\u043b\u0435\u0434\u0443\u0435\u0442 \u0432\u044b\u0431\u0438\u0440\u0430\u0442\u044c \u0432 \u0434\u0438\u0430\u043f\u0430\u0437\u043e\u043d\u0435 50\u2013200.<\/p>\n<p>5) \u0421\u043a\u043e\u0440\u043e\u0441\u0442\u044c \u0432\u0440\u0430\u0449\u0435\u043d\u0438\u044f \u0448\u043d\u0435\u043a\u0430: \u043f\u043e\u0441\u043b\u0435 \u0440\u0435\u0433\u0443\u043b\u0438\u0440\u043e\u0432\u043a\u0438 \u0441\u043a\u043e\u0440\u043e\u0441\u0442\u0438 \u0448\u043d\u0435\u043a\u0430 \u0432 \u0441\u043e\u0447\u0435\u0442\u0430\u043d\u0438\u0438 \u0441 \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u043e\u0439 \u043d\u0435 \u0441\u043b\u0435\u0434\u0443\u0435\u0442 \u0447\u0430\u0441\u0442\u043e \u0438\u0437\u043c\u0435\u043d\u044f\u0442\u044c \u0435\u0451 \u0432 \u043f\u0440\u043e\u0446\u0435\u0441\u0441\u0435 \u044d\u043a\u0441\u0442\u0440\u0443\u0437\u0438\u0438 \u0441\u043c\u043e\u043b\u044b FEP; \u043f\u0440\u0438 \u043d\u0435\u043e\u0431\u0445\u043e\u0434\u0438\u043c\u043e\u0441\u0442\u0438 \u0440\u0435\u0433\u0443\u043b\u0438\u0440\u0443\u0439\u0442\u0435 \u0435\u0451 \u043d\u0435\u0437\u043d\u0430\u0447\u0438\u0442\u0435\u043b\u044c\u043d\u043e.<\/p>\n<p>6) \u0422\u0435\u0440\u043c\u043e\u0438\u0437\u043e\u043b\u044f\u0446\u0438\u044f \u0432\u044b\u0445\u043e\u0434\u043d\u043e\u0433\u043e \u043e\u0442\u0432\u0435\u0440\u0441\u0442\u0438\u044f \u0444\u043e\u0440\u043c\u044b: \u0437\u043e\u043d\u0430 \u0442\u0435\u0440\u043c\u043e\u0438\u0437\u043e\u043b\u044f\u0446\u0438\u0438 \u0434\u043e\u043b\u0436\u043d\u0430 \u043e\u0445\u0432\u0430\u0442\u044b\u0432\u0430\u0442\u044c \u0432\u0441\u044e \u0437\u043e\u043d\u0443 \u0432\u044b\u0442\u044f\u0436\u043a\u0438, \u0430 \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0430 \u0442\u0435\u0440\u043c\u043e\u0438\u0437\u043e\u043b\u044f\u0446\u0438\u0438 \u0434\u043e\u043b\u0436\u043d\u0430 \u0441\u043e\u0441\u0442\u0430\u0432\u043b\u044f\u0442\u044c 350\u2013380 \u00b0C, \u0447\u0442\u043e\u0431\u044b \u0438\u0437\u0431\u0435\u0436\u0430\u0442\u044c \u043e\u0431\u0440\u0430\u0437\u043e\u0432\u0430\u043d\u0438\u044f \u043d\u0430\u043f\u0440\u044f\u0436\u0435\u043d\u0438\u0439 \u0438\u0437-\u0437\u0430 \u0432\u043d\u0435\u0437\u0430\u043f\u043d\u043e\u0433\u043e \u043e\u0445\u043b\u0430\u0436\u0434\u0435\u043d\u0438\u044f \u043f\u043e\u0432\u0435\u0440\u0445\u043d\u043e\u0441\u0442\u0438 \u043a\u043e\u043d\u0443\u0441\u0430 FEP \u0434\u043e \u0435\u0433\u043e \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u044f, \u0447\u0442\u043e \u043f\u0440\u0438\u0432\u0435\u0434\u0451\u0442 \u043a \u0440\u0430\u0441\u0442\u0440\u0435\u0441\u043a\u0438\u0432\u0430\u043d\u0438\u044e \u0438\u0437\u043e\u043b\u044f\u0446\u0438\u0438.<\/p>\n<p>\u0424\u043e\u0440\u043c\u044b \u043f\u0440\u043e\u0434\u0443\u043a\u0442\u0430 \u043f\u0435\u0440\u0435\u0434 \u043f\u0435\u0440\u0435\u0440\u0430\u0431\u043e\u0442\u043a\u043e\u0439 \u0438 \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u0435\u043c \u0441\u043c\u043e\u043b\u044b FEP:<\/p>\n<p>1. \u0413\u0440\u0430\u043d\u0443\u043b\u044b, \u0438\u0441\u043f\u043e\u043b\u044c\u0437\u0443\u0435\u043c\u044b\u0435 \u0434\u043b\u044f \u044d\u043a\u0441\u0442\u0440\u0443\u0437\u0438\u043e\u043d\u043d\u043e\u0433\u043e \u0438 \u043b\u0438\u0442\u044c\u0435\u0432\u043e\u0433\u043e \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u044f;<\/p>\n<p>2. \u0414\u0438\u0441\u043f\u0435\u0440\u0441\u0438\u044f, \u0438\u0441\u043f\u043e\u043b\u044c\u0437\u0443\u0435\u043c\u0430\u044f \u0434\u043b\u044f \u043f\u0440\u043e\u043f\u0438\u0442\u043a\u0438 \u0438 \u043d\u0430\u043d\u0435\u0441\u0435\u043d\u0438\u044f \u043f\u043e\u043a\u0440\u044b\u0442\u0438\u0439;<\/p>\n<p>3. \u041f\u043e\u0440\u043e\u0448\u043a\u043e\u0432\u044b\u0439 \u043c\u0430\u0442\u0435\u0440\u0438\u0430\u043b, \u0438\u0441\u043f\u043e\u043b\u044c\u0437\u0443\u0435\u043c\u044b\u0439 \u0434\u043b\u044f \u044d\u043b\u0435\u043a\u0442\u0440\u043e\u0441\u0442\u0430\u0442\u0438\u0447\u0435\u0441\u043a\u043e\u0433\u043e \u043d\u0430\u043f\u044b\u043b\u0435\u043d\u0438\u044f.<\/p>\n<p>\u041d\u0438\u0436\u0435 \u043c\u044b \u0432 \u043e\u0441\u043d\u043e\u0432\u043d\u043e\u043c \u0440\u0430\u0441\u0441\u043c\u043e\u0442\u0440\u0438\u043c \u043d\u0435\u0441\u043a\u043e\u043b\u044c\u043a\u043e \u043c\u0435\u0442\u043e\u0434\u043e\u0432 \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u044f \u0438 \u043f\u0435\u0440\u0435\u0440\u0430\u0431\u043e\u0442\u043a\u0438 FEP.<\/p>\n<p>1. \u0424\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u0435 \u044d\u043a\u0441\u0442\u0440\u0443\u0437\u0438\u0435\u0439 \u0440\u0430\u0441\u043f\u043b\u0430\u0432\u0430<\/p>\n<p>2. \u041a\u043e\u043c\u043f\u0440\u0435\u0441\u0441\u0438\u043e\u043d\u043d\u043e\u0435 \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u0435: \u043d\u0430\u0433\u0440\u0435\u0432, \u0441\u043e\u0437\u0434\u0430\u043d\u0438\u0435 \u0434\u0430\u0432\u043b\u0435\u043d\u0438\u044f \u0438 \u043f\u043b\u0430\u0441\u0442\u0438\u0444\u0438\u043a\u0430\u0446\u0438\u044f; \u043e\u0445\u043b\u0430\u0436\u0434\u0435\u043d\u0438\u0435, \u0441\u043e\u0437\u0434\u0430\u043d\u0438\u0435 \u0434\u0430\u0432\u043b\u0435\u043d\u0438\u044f \u0434\u043b\u044f \u043f\u0440\u0438\u0434\u0430\u043d\u0438\u044f \u0444\u043e\u0440\u043c\u044b<\/p>\n<p>3. \u0424\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u0435 \u0432\u044b\u0434\u0443\u0432\u0430\u043d\u0438\u0435\u043c<\/p>\n<p>4. \u0412\u0430\u043a\u0443\u0443\u043c\u043d\u043e\u0435 \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u0435<\/p>\n<p>5. \u041b\u0438\u0442\u044c\u0435\u0432\u043e\u0435 \u0444\u043e\u0440\u043c\u043e\u0432\u0430\u043d\u0438\u0435<\/p>\n<p>6. \u041d\u0430\u043d\u0435\u0441\u0435\u043d\u0438\u0435 \u043f\u043e\u043a\u0440\u044b\u0442\u0438\u0439<\/p>\n<p>7. \u042d\u043b\u0435\u043a\u0442\u0440\u043e\u0441\u0442\u0430\u0442\u0438\u0447\u0435\u0441\u043a\u043e\u0435 \u043d\u0430\u043f\u044b\u043b\u0435\u043d\u0438\u0435<\/p>\n<p>BOSS Sealing Solutions \u2014 \u043f\u0440\u043e\u0444\u0435\u0441\u0441\u0438\u043e\u043d\u0430\u043b\u044c\u043d\u0430\u044f \u043a\u043e\u043c\u043f\u0430\u043d\u0438\u044f \u043f\u043e \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0443 \u0443\u043f\u043b\u043e\u0442\u043d\u0435\u043d\u0438\u0439, \u0432\u044b\u043f\u0443\u0441\u043a\u0430\u044e\u0449\u0430\u044f \u0442\u0440\u0443\u0431\u043a\u0438 FEP \u0440\u0430\u0437\u043b\u0438\u0447\u043d\u044b\u0445 \u0440\u0430\u0437\u043c\u0435\u0440\u043e\u0432, \u0442\u0440\u0443\u0431\u043a\u0438 PFA, \u0438\u043d\u043a\u0430\u043f\u0441\u0443\u043b\u0438\u0440\u043e\u0432\u0430\u043d\u043d\u044b\u0435 \u043a\u043e\u043b\u044c\u0446\u0430 \u043a\u0440\u0443\u0433\u043b\u043e\u0433\u043e \u0441\u0435\u0447\u0435\u043d\u0438\u044f FEP, \u0432\u044b\u0441\u043e\u043a\u043e\u0435 \u043a\u0430\u0447\u0435\u0441\u0442\u0432\u043e, \u043b\u0443\u0447\u0448\u0430\u044f \u0446\u0435\u043d\u0430.<\/p>\n<p>\u043f\u043e \u043b\u044e\u0431\u044b\u043c \u0432\u043e\u043f\u0440\u043e\u0441\u0430\u043c \u043e \u0442\u0440\u0443\u0431\u043a\u0430\u0445 FEP \u0438 \u043a\u043e\u043b\u044c\u0446\u0430\u0445 \u043a\u0440\u0443\u0433\u043b\u043e\u0433\u043e \u0441\u0435\u0447\u0435\u043d\u0438\u044f FEP, \u043f\u043e\u0436\u0430\u043b\u0443\u0439\u0441\u0442\u0430, \u043e\u0442\u043f\u0440\u0430\u0432\u043b\u044f\u0439\u0442\u0435 \u043f\u0438\u0441\u044c\u043c\u043e \u043d\u0430 <a href=\"mailto:sales@bosssealing.com\">sales@bosssealing.com<\/a><\/p>\n<\/div>","protected":false},"excerpt":{"rendered":"<p>FEP manufacturing process FEP manufacturing process FEP has better processing performance. The following is what needs to be prepared before extrusion of FEP pipe: 1) Feeding: Before FEP extrusion, pre-bake at 120\u2103 for about 3h. 2) Conductive core preheating: In order to ensure the uniform temperature inside and outside the extruded FEP insulation layer, the [&hellip;]<\/p>\n","protected":false},"author":1,"featured_media":0,"comment_status":"open","ping_status":"open","sticky":false,"template":"","format":"standard","meta":{"_monsterinsights_skip_tracking":false,"footnotes":""},"categories":[1],"tags":[],"class_list":["post-218","post","type-post","status-publish","format-standard","hentry","category-news"],"aioseo_notices":[],"aioseo_head":"\n\t\t<!-- All in One SEO 5.0.4 - aioseo.com -->\n\t<meta name=\"description\" content=\"FEP manufacturing process FEP manufacturing process FEP has better processing performance. The following is what needs to be prepared before extrusion of FEP pipe: 1) Feeding: Before FEP extrusion, pre-bake at 120\u2103 for about 3h. 2) Conductive core preheating: In order to ensure the uniform temperature inside and outside the extruded FEP insulation layer, the\" \/>\n\t<meta name=\"robots\" content=\"max-image-preview:large\" \/>\n\t<meta name=\"author\" content=\"boss\"\/>\n\t<link rel=\"canonical\" href=\"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/\" \/>\n\t\t<meta name=\"generator\" content=\"All in One SEO (AIOSEO) 5.0.4\" \/>\n\t\t<meta property=\"og:locale\" content=\"ru_RU\" \/>\n\t\t<meta property=\"og:site_name\" content=\"BOSS Sealing Solutions - Hydraulic seal and pneumatic seal factory\" \/>\n\t\t<meta property=\"og:type\" content=\"article\" \/>\n\t\t<meta property=\"og:title\" content=\"FEP manufacturing process - BOSS Sealing Solutions\" \/>\n\t\t<meta property=\"og:description\" content=\"FEP manufacturing process FEP manufacturing process FEP has better processing performance. The following is what needs to be prepared before extrusion of FEP pipe: 1) Feeding: Before FEP extrusion, pre-bake at 120\u2103 for about 3h. 2) Conductive core preheating: In order to ensure the uniform temperature inside and outside the extruded FEP insulation layer, the\" \/>\n\t\t<meta property=\"og:url\" content=\"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/\" \/>\n\t\t<meta property=\"og:image\" content=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png\" \/>\n\t\t<meta property=\"og:image:secure_url\" content=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png\" \/>\n\t\t<meta property=\"article:published_time\" content=\"2021-06-09T03:09:36+00:00\" \/>\n\t\t<meta property=\"article:modified_time\" content=\"2023-07-18T06:18:30+00:00\" \/>\n\t\t<meta name=\"twitter:card\" content=\"summary_large_image\" \/>\n\t\t<meta name=\"twitter:title\" content=\"FEP manufacturing process - BOSS Sealing Solutions\" \/>\n\t\t<meta name=\"twitter:description\" content=\"FEP manufacturing process FEP manufacturing process FEP has better processing performance. The following is what needs to be prepared before extrusion of FEP pipe: 1) Feeding: Before FEP extrusion, pre-bake at 120\u2103 for about 3h. 2) Conductive core preheating: In order to ensure the uniform temperature inside and outside the extruded FEP insulation layer, the\" \/>\n\t\t<meta name=\"twitter:image\" content=\"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png\" \/>\n\t\t<script type=\"application\/ld+json\" class=\"aioseo-schema\">\n\t\t\t{\"@context\":\"https:\\\/\\\/schema.org\",\"@graph\":[{\"@type\":\"BlogPosting\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#blogposting\",\"name\":\"FEP manufacturing process - BOSS Sealing Solutions\",\"headline\":\"FEP manufacturing process\",\"author\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/author\\\/boss\\\/#author\"},\"publisher\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/#organization\"},\"image\":{\"@type\":\"ImageObject\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/wp-content\\\/uploads\\\/2023\\\/07\\\/logo.png\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/#articleImage\",\"width\":1744,\"height\":555,\"caption\":\"BOSS Sealing Solutions\"},\"datePublished\":\"2021-06-09T11:09:36+08:00\",\"dateModified\":\"2023-07-18T14:18:30+08:00\",\"inLanguage\":\"ru-RU\",\"mainEntityOfPage\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#webpage\"},\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#webpage\"},\"articleSection\":\"Knowledge Base\"},{\"@type\":\"BreadcrumbList\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#breadcrumblist\",\"itemListElement\":[{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/#listItem\",\"position\":1,\"name\":\"Home\",\"item\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/\",\"nextItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/category\\\/news\\\/#listItem\",\"name\":\"Knowledge Base\"}},{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/category\\\/news\\\/#listItem\",\"position\":2,\"name\":\"Knowledge Base\",\"item\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/category\\\/news\\\/\",\"nextItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#listItem\",\"name\":\"FEP manufacturing process\"},\"previousItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/#listItem\",\"name\":\"Home\"}},{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#listItem\",\"position\":3,\"name\":\"FEP manufacturing process\",\"previousItem\":{\"@type\":\"ListItem\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/category\\\/news\\\/#listItem\",\"name\":\"Knowledge Base\"}}]},{\"@type\":\"Organization\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/#organization\",\"name\":\"BOSS Sealing Solutions\",\"description\":\"Hydraulic seal and pneumatic seal factory\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/\",\"email\":\"sales@bosssealing.com\",\"telephone\":\"+86 13392768056\",\"logo\":{\"@type\":\"ImageObject\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/wp-content\\\/uploads\\\/2023\\\/07\\\/logo.png\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#organizationLogo\",\"width\":1744,\"height\":555,\"caption\":\"BOSS Sealing Solutions\"},\"image\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#organizationLogo\"}},{\"@type\":\"Person\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/author\\\/boss\\\/#author\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/author\\\/boss\\\/\",\"name\":\"boss\"},{\"@type\":\"WebPage\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#webpage\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/\",\"name\":\"FEP manufacturing process - BOSS Sealing Solutions\",\"description\":\"FEP manufacturing process FEP manufacturing process FEP has better processing performance. The following is what needs to be prepared before extrusion of FEP pipe: 1) Feeding: Before FEP extrusion, pre-bake at 120\\u2103 for about 3h. 2) Conductive core preheating: In order to ensure the uniform temperature inside and outside the extruded FEP insulation layer, the\",\"inLanguage\":\"ru-RU\",\"isPartOf\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/#website\"},\"breadcrumb\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/fep-manufacturing-process\\\/#breadcrumblist\"},\"author\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/author\\\/boss\\\/#author\"},\"creator\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/author\\\/boss\\\/#author\"},\"datePublished\":\"2021-06-09T11:09:36+08:00\",\"dateModified\":\"2023-07-18T14:18:30+08:00\"},{\"@type\":\"WebSite\",\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/#website\",\"url\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/\",\"name\":\"BOSS Sealing Solutions\",\"alternateName\":\"BOSS Sealing\",\"description\":\"Hydraulic seal and pneumatic seal factory\",\"inLanguage\":\"ru-RU\",\"publisher\":{\"@id\":\"https:\\\/\\\/www.bosssealing.com\\\/ru\\\/#organization\"}}]}\n\t\t<\/script>\n\t\t<!-- All in One SEO -->\n\n","aioseo_head_json":{"title":"\u041f\u0440\u043e\u0446\u0435\u0441\u0441 \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0430 FEP - BOSS Sealing Solutions","description":"\u041f\u0440\u043e\u0446\u0435\u0441\u0441 \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0430 FEP \u041f\u0440\u043e\u0446\u0435\u0441\u0441 \u043f\u0440\u043e\u0438\u0437\u0432\u043e\u0434\u0441\u0442\u0432\u0430 FEP FEP \u043e\u0431\u043b\u0430\u0434\u0430\u0435\u0442 \u043b\u0443\u0447\u0448\u0438\u043c\u0438 \u0442\u0435\u0445\u043d\u043e\u043b\u043e\u0433\u0438\u0447\u0435\u0441\u043a\u0438\u043c\u0438 \u0441\u0432\u043e\u0439\u0441\u0442\u0432\u0430\u043c\u0438. \u041d\u0438\u0436\u0435 \u043f\u0435\u0440\u0435\u0447\u0438\u0441\u043b\u0435\u043d\u043e \u0442\u043e, \u0447\u0442\u043e \u043d\u0435\u043e\u0431\u0445\u043e\u0434\u0438\u043c\u043e \u043f\u043e\u0434\u0433\u043e\u0442\u043e\u0432\u0438\u0442\u044c \u043f\u0435\u0440\u0435\u0434 \u044d\u043a\u0441\u0442\u0440\u0443\u0437\u0438\u0435\u0439 \u0442\u0440\u0443\u0431\u044b \u0438\u0437 FEP: 1) \u041f\u043e\u0434\u0430\u0447\u0430: \u043f\u0435\u0440\u0435\u0434 \u044d\u043a\u0441\u0442\u0440\u0443\u0437\u0438\u0435\u0439 FEP \u0432\u044b\u043f\u043e\u043b\u043d\u0438\u0442\u0435 \u043f\u0440\u0435\u0434\u0432\u0430\u0440\u0438\u0442\u0435\u043b\u044c\u043d\u044b\u0439 \u043f\u0440\u043e\u0433\u0440\u0435\u0432 \u043f\u0440\u0438 120\u2103 \u0432 \u0442\u0435\u0447\u0435\u043d\u0438\u0435 \u043f\u0440\u0438\u043c\u0435\u0440\u043d\u043e 3 \u0447. 2) \u041f\u0440\u0435\u0434\u0432\u0430\u0440\u0438\u0442\u0435\u043b\u044c\u043d\u044b\u0439 \u043d\u0430\u0433\u0440\u0435\u0432 \u0442\u043e\u043a\u043e\u043f\u0440\u043e\u0432\u043e\u0434\u044f\u0449\u0435\u0439 \u0436\u0438\u043b\u044b: \u0447\u0442\u043e\u0431\u044b \u043e\u0431\u0435\u0441\u043f\u0435\u0447\u0438\u0442\u044c \u0440\u0430\u0432\u043d\u043e\u043c\u0435\u0440\u043d\u0443\u044e \u0442\u0435\u043c\u043f\u0435\u0440\u0430\u0442\u0443\u0440\u0443 \u0432\u043d\u0443\u0442\u0440\u0438 \u0438 \u0441\u043d\u0430\u0440\u0443\u0436\u0438 \u044d\u043a\u0441\u0442\u0440\u0443\u0434\u0438\u0440\u043e\u0432\u0430\u043d\u043d\u043e\u0433\u043e \u0438\u0437\u043e\u043b\u044f\u0446\u0438\u043e\u043d\u043d\u043e\u0433\u043e \u0441\u043b\u043e\u044f FEP,","canonical_url":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/","robots":"max-image-preview:large","keywords":"","webmasterTools":{"miscellaneous":""},"schema":{"@context":"https:\/\/schema.org","@graph":[{"@type":"BlogPosting","@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#blogposting","name":"FEP manufacturing process - BOSS Sealing Solutions","headline":"FEP manufacturing process","author":{"@id":"https:\/\/www.bosssealing.com\/ru\/author\/boss\/#author"},"publisher":{"@id":"https:\/\/www.bosssealing.com\/ru\/#organization"},"image":{"@type":"ImageObject","url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","@id":"https:\/\/www.bosssealing.com\/ru\/#articleImage","width":1744,"height":555,"caption":"BOSS Sealing Solutions"},"datePublished":"2021-06-09T11:09:36+08:00","dateModified":"2023-07-18T14:18:30+08:00","inLanguage":"ru-RU","mainEntityOfPage":{"@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#webpage"},"isPartOf":{"@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#webpage"},"articleSection":"Knowledge Base"},{"@type":"BreadcrumbList","@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#breadcrumblist","itemListElement":[{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/ru\/#listItem","position":1,"name":"Home","item":"https:\/\/www.bosssealing.com\/ru\/","nextItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/ru\/category\/news\/#listItem","name":"Knowledge Base"}},{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/ru\/category\/news\/#listItem","position":2,"name":"Knowledge Base","item":"https:\/\/www.bosssealing.com\/ru\/category\/news\/","nextItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#listItem","name":"FEP manufacturing process"},"previousItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/ru\/#listItem","name":"Home"}},{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#listItem","position":3,"name":"FEP manufacturing process","previousItem":{"@type":"ListItem","@id":"https:\/\/www.bosssealing.com\/ru\/category\/news\/#listItem","name":"Knowledge Base"}}]},{"@type":"Organization","@id":"https:\/\/www.bosssealing.com\/ru\/#organization","name":"BOSS Sealing Solutions","description":"Hydraulic seal and pneumatic seal factory","url":"https:\/\/www.bosssealing.com\/ru\/","email":"sales@bosssealing.com","telephone":"+86 13392768056","logo":{"@type":"ImageObject","url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#organizationLogo","width":1744,"height":555,"caption":"BOSS Sealing Solutions"},"image":{"@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#organizationLogo"}},{"@type":"Person","@id":"https:\/\/www.bosssealing.com\/ru\/author\/boss\/#author","url":"https:\/\/www.bosssealing.com\/ru\/author\/boss\/","name":"boss"},{"@type":"WebPage","@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#webpage","url":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/","name":"FEP manufacturing process - BOSS Sealing Solutions","description":"FEP manufacturing process FEP manufacturing process FEP has better processing performance. The following is what needs to be prepared before extrusion of FEP pipe: 1) Feeding: Before FEP extrusion, pre-bake at 120\u2103 for about 3h. 2) Conductive core preheating: In order to ensure the uniform temperature inside and outside the extruded FEP insulation layer, the","inLanguage":"ru-RU","isPartOf":{"@id":"https:\/\/www.bosssealing.com\/ru\/#website"},"breadcrumb":{"@id":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/#breadcrumblist"},"author":{"@id":"https:\/\/www.bosssealing.com\/ru\/author\/boss\/#author"},"creator":{"@id":"https:\/\/www.bosssealing.com\/ru\/author\/boss\/#author"},"datePublished":"2021-06-09T11:09:36+08:00","dateModified":"2023-07-18T14:18:30+08:00"},{"@type":"WebSite","@id":"https:\/\/www.bosssealing.com\/ru\/#website","url":"https:\/\/www.bosssealing.com\/ru\/","name":"BOSS Sealing Solutions","alternateName":"BOSS Sealing","description":"Hydraulic seal and pneumatic seal factory","inLanguage":"ru-RU","publisher":{"@id":"https:\/\/www.bosssealing.com\/ru\/#organization"}}]},"og:locale":"ru_RU","og:site_name":"BOSS Sealing Solutions - Hydraulic seal and pneumatic seal factory","og:type":"article","og:title":"FEP manufacturing process - BOSS Sealing Solutions","og:description":"FEP manufacturing process FEP manufacturing process FEP has better processing performance. The following is what needs to be prepared before extrusion of FEP pipe: 1) Feeding: Before FEP extrusion, pre-bake at 120\u2103 for about 3h. 2) Conductive core preheating: In order to ensure the uniform temperature inside and outside the extruded FEP insulation layer, the","og:url":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/","og:image":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","og:image:secure_url":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png","article:published_time":"2021-06-09T03:09:36+00:00","article:modified_time":"2023-07-18T06:18:30+00:00","twitter:card":"summary_large_image","twitter:title":"FEP manufacturing process - BOSS Sealing Solutions","twitter:description":"FEP manufacturing process FEP manufacturing process FEP has better processing performance. The following is what needs to be prepared before extrusion of FEP pipe: 1) Feeding: Before FEP extrusion, pre-bake at 120\u2103 for about 3h. 2) Conductive core preheating: In order to ensure the uniform temperature inside and outside the extruded FEP insulation layer, the","twitter:image":"https:\/\/www.bosssealing.com\/wp-content\/uploads\/2023\/07\/logo.png"},"aioseo_meta_data":{"post_id":"218","title":"","description":"","keywords":"","keyphrases":"","primary_term":"","canonical_url":"","og_title":"","og_description":"","og_object_type":"default","og_image_type":"default","og_image_url":"","og_image_width":"0","og_image_height":"0","og_image_custom_url":"","og_image_custom_fields":"","og_video":"","og_custom_url":"","og_article_section":"","og_article_tags":"","twitter_use_og":false,"twitter_card":"default","twitter_image_type":"default","twitter_image_url":"","twitter_image_custom_url":"","twitter_image_custom_fields":"","twitter_title":"","twitter_description":"","schema":{"blockGraphs":[],"customGraphs":[],"default":{"data":{"Article":[],"Course":[],"Dataset":[],"FAQPage":[],"Movie":[],"Person":[],"Product":[],"ProductReview":[],"Car":[],"Recipe":[],"Service":[],"SoftwareApplication":[],"WebPage":[]},"graphName":"","isEnabled":true},"graphs":[]},"schema_type":"default","schema_type_options":"","pillar_content":false,"robots_default":true,"robots_noindex":false,"robots_noarchive":false,"robots_nosnippet":false,"robots_nofollow":false,"robots_noimageindex":false,"robots_noodp":false,"robots_notranslate":false,"robots_max_snippet":"0","robots_max_videopreview":"0","robots_max_imagepreview":"large","priority":0,"frequency":"","local_seo":"","breadcrumb_settings":null,"limit_modified_date":false,"ai":null,"created":"2023-07-18 06:32:31","updated":"2025-07-29 01:50:56","seo_analyzer_scan_date":null,"focus_keyword":null,"additional_keywords":null,"truseo_locale":null},"aioseo_breadcrumb":"<div class=\"aioseo-breadcrumbs\"><span class=\"aioseo-breadcrumb\">\n\t\t\t<a href=\"https:\/\/www.bosssealing.com\/ru\/\" title=\"Home\">Home<\/a>\n\t\t<\/span><span class=\"aioseo-breadcrumb-separator\">\u00bb<\/span><span class=\"aioseo-breadcrumb\">\n\t\t\t<a href=\"https:\/\/www.bosssealing.com\/ru\/category\/news\/\" title=\"Knowledge Base\">Knowledge Base<\/a>\n\t\t<\/span><span class=\"aioseo-breadcrumb-separator\">\u00bb<\/span><span class=\"aioseo-breadcrumb\">\n\t\t\tFEP manufacturing process\n\t\t<\/span><\/div>","aioseo_breadcrumb_json":[{"label":"Home","link":"https:\/\/www.bosssealing.com\/ru\/"},{"label":"Knowledge Base","link":"https:\/\/www.bosssealing.com\/ru\/category\/news\/"},{"label":"FEP manufacturing process","link":"https:\/\/www.bosssealing.com\/ru\/fep-manufacturing-process\/"}],"_links":{"self":[{"href":"https:\/\/www.bosssealing.com\/ru\/wp-json\/wp\/v2\/posts\/218","targetHints":{"allow":["GET"]}}],"collection":[{"href":"https:\/\/www.bosssealing.com\/ru\/wp-json\/wp\/v2\/posts"}],"about":[{"href":"https:\/\/www.bosssealing.com\/ru\/wp-json\/wp\/v2\/types\/post"}],"author":[{"embeddable":true,"href":"https:\/\/www.bosssealing.com\/ru\/wp-json\/wp\/v2\/users\/1"}],"replies":[{"embeddable":true,"href":"https:\/\/www.bosssealing.com\/ru\/wp-json\/wp\/v2\/comments?post=218"}],"version-history":[{"count":0,"href":"https:\/\/www.bosssealing.com\/ru\/wp-json\/wp\/v2\/posts\/218\/revisions"}],"wp:attachment":[{"href":"https:\/\/www.bosssealing.com\/ru\/wp-json\/wp\/v2\/media?parent=218"}],"wp:term":[{"taxonomy":"category","embeddable":true,"href":"https:\/\/www.bosssealing.com\/ru\/wp-json\/wp\/v2\/categories?post=218"},{"taxonomy":"post_tag","embeddable":true,"href":"https:\/\/www.bosssealing.com\/ru\/wp-json\/wp\/v2\/tags?post=218"}],"curies":[{"name":"wp","href":"https:\/\/api.w.org\/{rel}","templated":true}]}}